Subscriber access provided by University of South Dakota
Environmental Processes
Optimal design of sulfidated nanoscale zerovalent iron for enhanced trichloroethene degradation Sourjya Bhattacharjee, and Subhasis Ghoshal Environ. Sci. Technol., Just Accepted Manuscript • DOI: 10.1021/acs.est.8b02399 • Publication Date (Web): 06 Sep 2018 Downloaded from http://pubs.acs.org on September 6, 2018
Just Accepted “Just Accepted” manuscripts have been peer-reviewed and accepted for publication. They are posted online prior to technical editing, formatting for publication and author proofing. The American Chemical Society provides “Just Accepted” as a service to the research community to expedite the dissemination of scientific material as soon as possible after acceptance. “Just Accepted” manuscripts appear in full in PDF format accompanied by an HTML abstract. “Just Accepted” manuscripts have been fully peer reviewed, but should not be considered the official version of record. They are citable by the Digital Object Identifier (DOI®). “Just Accepted” is an optional service offered to authors. Therefore, the “Just Accepted” Web site may not include all articles that will be published in the journal. After a manuscript is technically edited and formatted, it will be removed from the “Just Accepted” Web site and published as an ASAP article. Note that technical editing may introduce minor changes to the manuscript text and/or graphics which could affect content, and all legal disclaimers and ethical guidelines that apply to the journal pertain. ACS cannot be held responsible for errors or consequences arising from the use of information contained in these “Just Accepted” manuscripts.
is published by the American Chemical Society. 1155 Sixteenth Street N.W., Washington, DC 20036 Published by American Chemical Society. Copyright © American Chemical Society. However, no copyright claim is made to original U.S. Government works, or works produced by employees of any Commonwealth realm Crown government in the course of their duties.
Page 1 of 24
Environmental Science & Technology
1
Optimal design of
2
sulfidated nanoscale zerovalent iron
3
for enhanced trichloroethene degradation *
4
Sourjya Bhattacharjee, Subhasis Ghoshal
5
Department of Civil Engineering, McGill University, Montreal, QC H3A 0C3, Canada
6 7
submitted to
8 9
Environmental Science & Technology
10 11 12 13 14 15 16
*Corresponding author phone: 514-398-6867; fax: 514-398-7361; email:
[email protected] 17 18 19 20 1 ACS Paragon Plus Environment
Environmental Science & Technology
Page 2 of 24
21
ABSTRACT:
22
Sulfidated nanoscale zerovalent iron (S-nZVI) has the potential to be a cost-effective remediation agent for a
23
wide range of environmental pollutants including chlorinated solvents. Various synthesis approaches have
24
yielded S-nZVI consisting of a Fe0 (or Fe0/S0) core and FeS shell, which are significantly more reactive to
25
trichloroethene (TCE) than nZVI. However, their reactivity is not as high as palladium-doped nZVI (Pd-
26
nZVI). We synthesized S-nZVI by co-precipitation of FeS and Fe0, using Na2S during borohydride reduction
27
of FeSO4 (S-nZVIco). This resulted in FeS structures bridging the nZVI core and the surface, as confirmed by
28
electron microscopy and X-ray analyses. TCE degradation capacity of up to 0.46 moles TCE/mole Fe0 was
29
obtained for S-nZVIco at high S loading, and was comparable to Pd-nZVI but 60% higher than the currently
30
most reactive S-nZVI in which FeS only coats the nZVI (S-nZVIpost). The high TCE degradation was due to
31
complete utilization of Fe0 (2 e-/mole Fe0) towards formation of acetylene. Although Pd-nZVI yielded 3 e-
32
/mole Fe0, TCE degradation was comparable because it reduced acetylene further to ethene and ethane.
33
Under Fe0 limited conditions, S-nZVIco TCE degradation rate was 16 times higher than Pd-nZVI (0.5 wt.%
34
Pd ), and 90 times higher than S-nZVIpost.
35
2 ACS Paragon Plus Environment
Page 3 of 24
Environmental Science & Technology
36
INTRODUCTION
37
Nanoscale zerovalent iron (nZVI) has been investigated extensively over the past several years for the
38
removal of a wide range of environmental contaminants such as heavy metals, chlorinated solvents,
39
pesticides and dyes.1, 2 Potential benefits arising from the nanoscale size, particularly higher contaminant
40
removal capacities and feasibility of injection in finer aquifer material containing subsurface zones
41
compared to micro-scale ZVI, has led to significant interest in nZVI-based in situ groundwater remediation.
42
However, removal of chlorinated organic contaminants such as trichloroethene (TCE) from water by nZVI is
43
limited due to its poor selectivity towards TCE and preferential reactions with water that generate
44
hydrogen.3,
45
improve reactivity of nZVI to TCE by enhancing TCE concentrations near the nZVI surface by sorption to
46
activated carbon, and leads to modest increases in TCE degradation rates.5 Doping the nZVI surface with
47
noble metals such as palladium (Pd-nZVI) has been effective in improving TCE degradation rates by several
48
orders of magnitude, due to the role of Pd0 as an electron conductor and hydrogenation catalyst.2,
49
However, major challenges with the use of Pd-nZVI for in situ groundwater remediation are its high cost,
50
and policy directives preventing its implementation, such as the precautionary principle in the EU Water
51
Framework Directive.8
52
Iron sulfide minerals such as iron monosulfide (FeS) are abundant, cheap and have good electron transfer
53
properties.9,
54
performance for contaminant remediation. The synthesis and use of sulfidated nZVI (S-nZVI) has been
55
explored in recent studies and has emerged as an important advancement towards the applicability of nZVI
56
for water treatment and environmental remediation. S-nZVI has demonstrated higher reactivity and removal
57
capacity towards a wide range of water contaminants such as metals11,
4
Composites of activated carbon and nZVI such as Carbo-Iron®, have been developed to
10
6, 7
Functionalization of nZVI with FeS is thus a cost-effective strategy to enhance nZVI
15-18
12
, pharmaceuticals13,
14
, and
58
halogenated organics
59
Kim et al.16 reported a 20-fold increase in the TCE degradation rate by S-nZVI compared to that achieved by
60
bare nZVI. The S-nZVI was synthesized by adding sodium dithionite as the sulfidation agent during
61
borohydride reduction of FeCl3, in a one-pot approach. This approach generates nanoparticles with a mixed
62
core of Fe0 and S0 surrounded by a shell of iron oxides and FeS.10, 12, 14, 16 However, the inclusion of dithionite
63
suppresses the crystallization of Fe0 and/or oxidizes Fe0, resulting in particles with low Fe0 content and thus
64
low TCE reduction capacities.19, 20 The Fe0 depletion provides a constraint on the extent of sulfidation that
65
can be achieved using dithionite towards a reactive S-nZVI. Kim et al.16 observed linear increases in the
66
pseudo first order TCE degradation rate constants (kobs) by S-nZVI, for dithionite concentrations up to 2.0
67
g/L, exceeding which the kobs decreased.
, than pure nZVI.
3 ACS Paragon Plus Environment
Environmental Science & Technology
Page 4 of 24
68
Rajajayavel et al.15 observed up to 40-fold increase in the TCE degradation rate by S-nZVI prepared by
69
contacting nZVI (synthesized by borohydride reduction of FeSO4) with aqueous solutions of sodium sulfide.
70
This two-step synthesis approach results in the formation of nanoparticles with a surface FeS layer and a Fe0
71
core.10, 11, 15 Na2S dissociates to form bisulfide ions in water which react with Fe0 to form FeS. However, use
72
of high doses of Na2S with the aim to incorporate more sulfur in the nanoparticle retarded the TCE reduction
73
rates. Rajajayavel et al.15 reported maximum TCE degradation rates between S/Fe molar ratios of 0.04 to
74
0.083 and proposed that the sulfide layer thickness on the Fe surface played a critical role in determining
75
TCE degradation rates. The authors also reported that S-nZVI had lower selectivity towards water resulting
76
in a 2.5 times lower hydrogen evolution rate compared to nZVI. In an earlier study, Fan et al.11 reported the
77
existence of an optimal S/Fe ratio of 0.056 wherein highest reduction and surface precipitation rates for
78
pertechnetate (anionic form of 99technetium) were observed. Han et al.21 also suggested the existence of an
79
optimum S/Fe ratio and reported that TCE degradation rate constants increased rapidly up to S/Fe ratio of
80
0.025 beyond which they plateaued off.
81
Despite the benefits demonstrated by sulfidation on reactivity of nZVI to TCE, studies to date have not been
82
able to achieve S-nZVI performance close to Pd-nZVI in terms of rates and extents of TCE degradation. For
83
instance, Ma et al.19 showed that S-nZVI removed 38% of the initial TCE over a 7-day period whereas Pd-
84
nZVI showed 100% removal in 2.5 hours. The authors prepared S-nZVI in a modified one-pot synthesis
85
approach by solely employing dithionite for simultaneous reduction and sulfidation of Fe2+ salt. The
86
resulting particles primarily consisted of Fe3O4 with low quantities of Fe0, and a shell of iron oxides and iron
87
sulfides. While both Pd0 and FeS are electron conductors to TCE, the intrinsic roles of Pd0 (hydrogenation
88
catalyst) and FeS (higher selectivity of TCE over water10, 15, 22, 23) are different with respect to improving
89
nZVI reactivity. Thus, approaches to further improve S-nZVI reactivity and use in groundwater remediation
90
are not obvious, and is a current area of interest.
91
Several studies, as discussed above, indicate that at high S/Fe ratios, the TCE degradation rate constants for
92
S-nZVI are diminished compared to the optimum. For S-nZVI where the Fe0 has not been depleted, this is
93
counter-intuitive because higher amounts of FeS should result in higher reactivity due to increased
94
conduction of electrons. Electron microscopy images of S-nZVI reveal the presence of laminar or flake-like
95
FeS structures primarily on the outside of the spherical Fe0 particles10-12 suggesting that at high S/Fe ratios,
96
there may only be limited contact of FeS to Fe0 . Therefore, we rationalized that by distributing FeS in the
97
nanoparticle such that it bridges the core to the exterior can maximize the association between Fe0 and FeS
98
and may result in increased TCE degradation rates. In this study we demonstrate that S-nZVI prepared in a
99
one-step approach using Na2S as the sulfidation agent yields such an architecture, while maintaining
100
sufficient amounts of Fe0. This results in an S-nZVI as reactive as Pd-nZVI, the most reactive form of nZVI. 4 ACS Paragon Plus Environment
Page 5 of 24
Environmental Science & Technology
101
We evaluated the TCE degradation rates, extents, and reaction end products in batch reactors, as well as
102
characterized changes in nanoparticle morphology and surface chemistry for S-nZVI synthesized through the
103
one-step approach. We compared its reactivity performance against the previously reported S-nZVI
104
synthesized through the two-step approach11,
105
experiments were carried out under Fe0 limited conditions and Fe0 excess conditions to obtain a more
106
complete understanding of the Fe0 reductive capacity.
107
MATERIALS AND METHODS
108
Chemicals and gases. FeSO4·7H2O (99%), NaBH4 (≥98.5%), Na2S (99%), palladium acetate (99%),
109
chloroethenes (vinyl chloride and cis 1, 2- & trans 1, 2- dichloroethene) and hexenes (cis 3- & trans 3-
110
≥95%) were obtained from Sigma-Aldrich. Gas standards of ethane, ethene, methane (99%, grade CP) and
111
1-, cis-, trans- butene (1000 ppm in N2) were obtained from Scotty Specialty Gases. Acetylene (99%) was
112
obtained from Praxair Inc. Methanol (99%) was purchased from Fisher Scientific. Water used in experiments
113
was double deionized.
114
Synthesis of nZVI. Bare nZVI particles were synthesized using a procedure described previously15 with
115
some modifications. Briefly, 1.3 M NaBH4 was added drop-wise at 5 mL/min using a syringe pump to a
116
continuously mixed aqueous solution of 0.3 M FeSO4·7H2O under anaerobic conditions followed by mixing
117
for 30 minutes. The resulting NZVI suspension was washed with methanol, dried under nitrogen, and stored
118
in an anaerobic chamber.
119
Synthesis of S-nZVIco. Sulfidated nZVI prepared by co-precipitation of iron sulfides and Fe0 in a one-step
120
approach is referred to herein as S-nZVIco, and is distinct from the two-step approach referred to herein as
121
post sulfidation (S-nZVIpost) in which sulfidation occurs after nZVI formation.
122
In the co-precipitation approach, aqueous solutions of NaBH4 (1.7 M) and Na2S (between 0.026 M to 0.64
123
M) were mixed together and then added drop-wise over a time period of 45 min, at 5 mL/min to a
124
continuously mixed aqueous solution of 0.3 M FeSO4·7H2O under anaerobic conditions, followed by 30
125
minutes of mixing. The resulting particles termed as S-nZVIco, were washed with methanol and dried in the
126
anaerobic chamber for 12 hours and then stored in the chamber in sealed vials until use. The sulfur
127
incorporated into the particles was measured and were 0.035, 0.05, 0.07, 0.1, 0.2, 0.3 and 0.4 as mole
128
fractions of S/Fe.
129
Synthesis of S-nZVIpost. The S/Fe mole ratios of S-nZVIco served as the molar dosing ratios ([S/Fe]dosed) in
130
the post-sulfidation approach. S-nZVIpost was prepared according to Rajajayavel et al.15 wherein, nZVI
131
particles were first prepared separately using the nZVI synthesis method described above, and then
15
as well as with Pd-nZVI and unamended nZVI. The
5 ACS Paragon Plus Environment
Environmental Science & Technology
Page 6 of 24
132
sulfidated directly in the vials used for TCE reaction experiments. This was done by adding different doses
133
of aqueous Na2S solutions to the nZVI suspensions equivalent to [S/Fe]dosed, followed by sonication of the
134
vials in a bath sonicator for 15 min. The uptake of sulfur by the particles was also measured. As discussed
135
later, complete uptake of sulfur did not take place, and S-nZVIpost suspensions contained undeposited
136
bisulfide ions.
137
Palladium doped nZVI (Pd-nZVI). An ethanolic solution of palladium acetate, at 1 wt. % of nZVI, was
138
added directly to nZVI suspensions in TCE reaction vials and sonicated for 15 min. All the Pd added was
139
deposited on the particles.
140
Reactivity studies. TCE degradation experiments were carried out in 60 mL vials crimp-sealed with butyl
141
rubber septa and samples were prepared in the anaerobic chamber and all solutions were purged with
142
nitrogen prior to handling. 100 µL TCE was added to reaction vials containing a total aqueous volume of
143
24.9 mL and 40 mg of nanoparticles.
144
Upon addition of TCE, a small globule of NAPL was formed. This provided a constant saturated aqueous
145
solution of TCE throughout the duration of the reactivity experiments. No measurable changes in the
146
headspace TCE concentrations occurred in the reactors, due to the saturated TCE solution and
147
stoichiometrically limited amounts of Fe0 compared to TCE. Thus TCE disappearance was tracked by
148
quantifying TCE degradation products with time and using a carbon mass balance approach as described in
149
our previous study.24 Calibration standards were prepared by adding known quantities of the gas standard in
150
the reactors set-up exactly like the reactivity systems.
151
Analytical methods. The mass of sulfur deposited on nZVI particles was measured using an ICP-OES
152
(PerkinElmer Optima 8300). The limit of detection for sulfur and iron was 25 ppb and 10 ppb measured at
153
wavelengths of 181 nm and 259 nm respectively. The nanoparticles were separated from solution using
154
centrifugation followed by magnetic separation and then the nanoparticles and supernatant were separately
155
acid digested in aqua regia (3:1 HCl: HNO3).
156
TCE degradation products were quantified periodically by injection of 300 µL reactor headspace into a gas
157
chromatograph (GC-FID and GC-MS). Details on GC, X-ray photoelectron spectroscopy (XPS) and
158
transmission electron microscopy coupled with energy dispersive spectroscopy (TEM-EDS) instrumentation
159
have been provided previously.24 Prior to measurement with XPS, S-nZVI samples were dried in an
160
anaerobic chamber. Before being analyzed with TEM, a drop of S-nZVI suspension was directly placed on
161
copper TEM grids and excess water was removed using a tissue. Fe0 content was measured using acid
162
digestion protocol mentioned elsewhere.25 The nanoparticles were acid digested in HCl and the liberated H2
163
gas was measured using a GC-TCD. Size and surface charge of nanoparticle suspensions were measured in a 6 ACS Paragon Plus Environment
Page 7 of 24
Environmental Science & Technology
164
Zetasizer Nano (Malvern). Nanoparticle suspensions were prepared at concentration of 150 ppm in 10 mM
165
NaHCO3 (pH 8.2), sonicated for 15 seconds and immediately analyzed to obtain a hydrodynamic diameter
166
(cumulant Z-average size) and zeta potential, with an acquisition time of 60 seconds. The particles were in
167
suspension throughout the duration of analysis. The refractive index of nanoparticles was set at 2.87.26
168
RESULTS AND DISCUSSION
169
Morphology of S-nZVIco is different from S-nZVIpost. A detailed comparison of the characteristics in
170
morphologies and surface chemistry of S-nZVIco and S-nZVIpost was carried out using TEM-EDS and XPS.
171
The representative TEM images of S-nZVIco and S-nZVIpost are shown in Figures 1a and 1b, respectively.
172
Overall, four distinct morphologies were observed in the images; needle and plate-like structures which were
173
often observed together (Type I), spherical particles in the size range of 100-150 nm with a rough surface
174
(Type II), small irregular particles in the size range of 20-30 nm (Type III), and particles in the size range of
175
50-200 nm with well-defined spherical boundaries (Type IV). S-nZVIco was abundant in Type I, Type II and
176
Type III morphologies whereas Type IV was rarely observed. In contrast, S-nZVIpost was primarily
177
composed of Type I and Type IV morphologies.
178 179
Figures 1a1-1a4 are blown up images of sections in Figure 1 that highlight the different morphologies
180
observed for S-nZVIco. As seen in Figures 1a1 and 1a2, Type I morphology consisted of laminar structures
181
which resembled a mix of needles and thin plates. Type I structures also appeared to be embedded within the
182
Type II particles. EDS analyses of Type I structures generated S signals along with Fe suggesting that they
183
were likely iron sulfides (Figure S1). Relatively small O signals were also present. Previous studies have
184
attributed the laminar shapes to FeS.11, 20, 27 Moreover, pure nano-FeS also shows a similar structure.28 XPS
185
analysis of S-nZVIco (Figure S2 and Table S1) showed predominance of FeS and presence of polysulfides
186
and sulfates to a lesser extent. This suggests that the Type I structures are FeS. The speciation of S-nZVIco
187
did not change at different [S/Fe]dosed(Table S1). Figure 1a2 shows the Type II morphology observed for S-
188
nZVIco and these were spherical particles with a granular appearance and surface roughness. EDS analysis of
189
the particle surface provided signals for Fe and S. The surface roughness of Type II particles may have been
190
caused due to the entrapment of Type I FeS structures. Figure 1a3 shows the Type III morphology which
191
were 20-30 nm irregularly shaped particles, the EDS for which provided Fe and S signals. The Type III
192
particles were observed to be enmeshed with Type I structures, usually at higher [S/Fe]dosed (Figure S1). The
193
presence of the smaller Type III particles likely resulted in the small increases in the BET surface area for S-
194
nZVIco with increasing [S/Fe]dosed (Table S2). Overall, the location of FeS structures were observed both
195
within and on the surface of the particles. In addition, the FeS structures formed extensive mesh like
196
networks with increasing [S/Fe]dosed (Figure S1), suggesting that multiple Fe0 rich sites may have been 7 ACS Paragon Plus Environment
Environmental Science & Technology
Page 8 of 24
197
bridged together in aqueous suspension, maximizing Fe0 and FeS contact. The structure of S-nZVIco is
198
distinct from the morphology of S-nZVI prepared in a one-pot approach using dithionite, wherein a defined
199
spherical core comprised of Fe0 and S0 was observed, with FeS flakes only on the outer shell for the latter10,
200
12
.
201 202
In contrast, S-nZVIpost particles were abundant in Type IV morphology. The particles generally had a smooth
203
spherical particle edge and were also observed to be associated with Type I FeS structures. However, the
204
FeS structures were located primarily on the outer surface of the spherical particles (Figure S3) unlike that
205
observed for S-nZVIco. XPS analysis of S-nZVIpost primarily showed the presence of FeS (Figure S4). Unlike
206
the XPS spectra for S-nZVIco (Figure S2), peaks for polysulfide or sulfate species in S-nZVIpost were not
207
observed. nZVI and Pd-nZVI employed in this study have been thoroughly characterized elsewhere.24 Both
208
nZVI and Pd-nZVI consisted of spherical particles with primary particle sizes in the range of 20-100 nm.
209 210
Analysis of aggregate size and surface charge of S-nZVIco and S-nZVIpost was also carried out at two
211
[S/Fe]dosed as shown in Table S3. S-nZVIco was present as smaller aggregate sizes than S-nZVIpost. For
212
example, at [S/Fe]dosed of 0.4, the mean aggregate diameter of S-nZVIco was 1.3±0.1 µm (PDI = 0.38),
213
whereas for S-nZVIpost, it was 4.4±0.4 µm (PDI = 0.5). The aggregate sizes of nZVI and Pd-nZVI were
214
similar at 7.2±0.8 µm (PDI = 0.7) and 7±0.5 µm (PDI = 0.6) respectively. We also observed that the zeta
215
potential of S-nZVIpost was higher (-37.1 mV at [S/Fe]dosed of 0.4) than S-nZVIco (-11.3 mV at [S/Fe]dosed of
216
0.4), nZVI (-6 mV) and Pd-nZVI (-6.5 mV). The differences could likely be related to the differences in the
217
surface characteristics, particularly the amounts and locations of sulfide and oxides deposited.
218 219
TCE degradation capacity of S-nZVIco is similar to Pd-nZVI and higher than S-nZVIpost. The extent of
220
TCE degradation achieved by S-nZVI is an important benchmark for assessing its remediation performance.
221
We evaluated the specific degradation capacity (defined in Equation 1) of nZVI, Pd-nZVI, S-nZVIco and S-
222
nZVIpost for TCE degradation and they are presented in Figure 2a. It should be noted that Pd-nZVI particles
223
did not contain any sulfur and their results are shown along with S-nZVI for comparison only.
224
, =
!"!#! $ %
(1)
225
The SDC was estimated by Equation 1, based on data from systems employing stoichiometrically excess
226
TCE mass compared to Fe0, for time points where no further TCE degradation was observed in each of the
227
reaction systems (Figure S5).
8 ACS Paragon Plus Environment
Page 9 of 24
Environmental Science & Technology
228
Figure 2a demonstrates that pure nZVI ([S/Fe]dosed = 0) achieved a low SDC of 0.01. This was likely due to
229
the preferential reactions of nZVI with water over TCE. Although nZVI only dechlorinated 5 µmoles of TCE
230
over 8 days during the degradation studies (Figure 2a, Figure S5c), we measured a total of 57 µmoles of H2
231
in the reactor in the same time period, suggesting reaction of nZVI with water was dominant compared to
232
reaction with TCE.
233
However as the [S/Fe]dosed increased from 0.035 to 0.1, the SDC of S-nZVIco increased substantially from
234
0.08±0.01 to 0.36±0.02. The increase in SDC was smaller between [S/Fe]dosed of 0.1 to 0.4, with a maximum
235
SDC of 0.46±0.02 being achieved at [S/Fe]dosed of 0.4. Conversely, S-nZVIpost achieved a maximum SDC of
236
only 0.28±0.02 within a similar range of [S/Fe]dosed. Pd-nZVI exhibited an SDC of 0.45±0.02 and varying the
237
Pd loading between 0.5 to 5 wt.% Pd did not significantly alter the SDC value (Figure S5c).
238
Among the three major TCE degradation products reported for Pd-nZVI and S-nZVI (acetylene, ethene and
239
ethane), a theoretical maximum SDC (SDCtheor,max) can be achieved when TCE is converted to the least
240
saturated product, i.e. acetylene. If 2 electrons per mole of Fe0 are available (Fe0 → Fe2+ + 2e-) and
241
acetylene is the major end product, then 2 moles of Fe0 are required to convert 1 mole TCE to acetylene
242
(& '() + 4 , + ' - → & '& + 3( , ), providing a SDCtheor,max of 0.5. However, if 3 electrons per mole of
243
Fe0 are available (Fe0 → Fe2+ + 2e- ; Fe2+ → Fe3+ + e-), then 1.33 moles of Fe0 are required to convert 1 mole
244
TCE to acetylene, providing a SDCtheor,max of 0.75.
245
In our previous study we observed that Pd-nZVI could provide up to 3 electrons per mole of Fe0 to
246
dechlorinate TCE.24 Therefore, as a first step towards understanding the differences in SDC observed in this
247
study, we analyzed the electrons available per mole of Fe0 for TCE degradation in the case of Pd-nZVI, S-
248
nZVIco and S-nZVIpost. This involved first the identification and quantification of the moles of end products
249
formed in the TCE degradation experiments (Table S4-S6). Subsequently, the electrons needed for formation
250
of those end products were calculated from stoichiometry. Thereafter, summation of electrons from the end
251
products yielded the total electrons used in the conversion of TCE by the nanoparticles. The total electrons
252
were then employed in electron balance calculation (Table S7), which confirmed that Pd-nZVI provided 3
253
electrons per mole of Fe0 for TCE dechlorination, whereas S-nZVIco and S-nZVIpost had 2 electrons per mole
254
of Fe0 available. The electron balance on average was ≥90%.
255
Despite the availability of lower number of electrons, S-nZVIco achieved a maximum SDC similar to Pd-
256
nZVI, between [S/Fe]dosed of 0.3 and 0.4, as seen in Figure 2a. We thus compared the end products generated
257
by Pd-nZVI and S-nZVIco to better understand how the available electrons were being utilized in the
258
degradation process. As shown in Figure 2b, Pd-nZVI primarily transformed TCE to ethene and ethane,
259
which accounted for 80% of the total dechlorination products. Whereas S-nZVIco degraded TCE 9 ACS Paragon Plus Environment
Environmental Science & Technology
Page 10 of 24
260
predominantly to acetylene (97% of total dechlorination products). Formation of ethene and ethane require 6
261
and 8 electrons per mole of Fe0 respectively, whereas acetylene requires only 4 electrons. Thus, the
262
generation of acetylene by S-nZVIco enabled it to achieve an SDC equivalent to that of Pd-nZVI despite
263
having fewer electrons available for TCE dechlorination. Thus, S-nZVIco achieves a maximum experimental
264
SDC (0.46) close to SDCtheor,max (0.5). However the experimental maximum SDC for Pd-nZVI (0.45) is 40%
265
lower than the SDCtheor,max (0.75). This was due to the inefficient electron distribution among the degradation
266
products by Pd-nZVI. Other than ethene and ethane, Pd-nZVI generates several byproducts including
267
dichlorethenes, which maybe undesirable in TCE degradation applications.
268
In contrast, S-nZVIpost did not achieve an SDC equivalent to S-nZVIco despite a similar availability of 2
269
electrons per mole of Fe0 and formation of similar degradation products. Additionally, the SDC for both S-
270
nZVIco and S-nZVIpost was dependent on the [S/Fe]dosed. For S-nZVIco and S-nZVIpost, FeS plays a critical
271
role in the shuttling of electrons from Fe0 to halogenated contaminants at the surface.14,
272
hypothesized that the amount of FeS associated with S-nZVIco and S-nZVIpost was different at different
273
[S/Fe]dosed which influenced the ability of the nanoparticles to release the available electrons per mole of Fe0
274
for TCE degradation. Therefore we measured the particle S/Fe ratio ([S/Fe]particle) to estimate the amounts of
275
FeS associated with S-nZVIco and S-nZVIpost at different [S/Fe]dosed. As shown in Figure 2c, S-nZVIpost
276
showed a limited uptake capacity for sulfur over the large range of [S/Fe]dosed employed. Relative to S-
277
nZVIco, the [S/Fe]particle values of S-nZVIpost were much lower. For instance, at the [S/Fe]dosed of 0.4, the
278
[S/Fe]particle for S-nZVIpost was only 0.05 whereas for S-nZVIco it was 0.4. This also implies that the S-
279
nZVIpost suspensions contained the remainder of the undeposited bisulfide ions, whereas the S-nZVIco
280
suspensions did not. The [S/Fe]particle for S-nZVIpost did not change between 15 min to 12 hrs of contact time
281
between nZVI and the Na2S solutions. Thus, the significantly lower amounts of sulfur associated with S-
282
nZVIpost is likely to have caused lower SDC in comparison to S-nZVIco. Furthermore by plotting the SDC’s
283
as a function of [S/Fe]particle (Figure 2d), S-nZVIpost and S-nZVIco displayed similar SDC values upto
284
[S/Fe]particle of 0.05, validating the hypothesis that amount of FeS associated with Fe0 influenced the SDC.
285
Increasing the [S/Fe]particle allowed for higher TCE transformation extents due to higher amounts of electrons
286
being extracted from the nanoparticle via FeS.
287
The difference in the amounts of sulfur in S-nZVIco and S-nZVIpost can be attributed to the distribution
288
pattern of FeS. As is seen in Figure 1b, FeS structures are associated with the S-nZVIpost particles, primarily
289
on the outer surface. The availability of FeS deposition sites (Fe0 and Fe-oxide sites) being limited to the
290
outer surface of S-nZVIpost likely caused the limited sulfur uptake.11 In contrast, for S-nZVIco FeS
291
precipitation occurs along with formation of Fe0 during the nanoparticle nucleation and growth phase. This
292
allows association of higher amounts of FeS with S-nZVIco through incorporation within the nanoparticles as
15, 18
We thus
10 ACS Paragon Plus Environment
Page 11 of 24
Environmental Science & Technology
293
well formation of FeS structures around the particles. We observed that with increases in the [S/Fe]dosed from
294
0 to 0.4, the initial Fe0 content (moles of initial Fe0 per mole of Fe) for S-nZVIco decreased from 0.82 to 0.4
295
respectively (Figure S5d). This is expected due to the stoichiometric consumption of Fe0 by HS- during FeS
296
formation. Interestingly, the initial Fe0 content of S-nZVIpost particles remained relatively unchanged for the
297
different [S/Fe] doses. This could be a result of the small [S/Fe]particle achieved by S-nZVIpost (Figure 2c) as
298
well as the replacement of only the surface Fe-oxides by FeS. Despite a lower Fe0 content, S-nZVIco is much
299
more reactive than S-nZVIpost. For instance, at [S/Fe]dosed of 0.4, S-nZVIco has an initial Fe0 content of 0.4
300
compared to S-nZVIpost which has 0.82. However S-nZVIco achieved an SDC of 0.46 compared to 0.28 of S-
301
nZVIpost. This demonstrates that Fe0 content or the sulfide dose alone does not determine TCE degradation
302
capacity and highlights the benefit of a rational particle design approach, wherein creating particle
303
architectures that maximize association between Fe0 and FeS can facilitate complete utilization of the nZVI
304
reductive power.
305
In a recent study, Gu et al.29 investigated the reactivity of sulfidated microscale zerovalent iron (S-mZVI) to
306
TCE. The authors reported that at [S/Fe]dosed of 0.1, the Fe0 in S-mZVI was completely consumed during
307
degradation reactions with TCE providing a maximum SDC of 0.39. Additionally, cis-DCE accounted for
308
16% of the total dechlorination products formed, and S-mZVI generated hydrogen during reactions with
309
TCE which accounted for 10% of the Fe0 consumption. Mackenzie et al.5 investigated the TCE degradation
310
extent of an nZVI and activated carbon composite, and an SDC of 0.2 was estimated from their study based
311
on the degradation products (mainly ethene) identified. In an earlier study, Liu et al.25 reported SDC’s of two
312
different nZVI, one containing a Fe-boron alloy which was catalytically active like bimetallic nZVI, and the
313
other being the commercially available RNIP which contained reduced sulfur species.30 Both particles
314
exhibited similar SDC’s of 0.25.
315
S-nZVIco has higher rates of TCE degradation than Pd-nZVI and S-nZVIpost. Along with quantifying
316
the extents of TCE degradation, we also evaluated the rates of degradation for each type of nanoparticle. The
317
TCE degradation profile over time was best fitted with a pseudo first order rate law (Figure S5 a and b) as
318
shown in the following integrated rate equation.
319
0# = 0 + 102 − 0 4 ,5678 #
320
In Equation 2, Mt is the moles of TCE in the reactor at any time t, M0 is the initial moles of TCE in the
321
reactor, Me is the moles of TCE in the reactor at the end of the degradation reaction, and kobs is the observed
322
pseudo-first-order TCE degradation rate constant (h-1). The observed rate constant was then normalized by
323
the particle BET surface areas (m2/g) and Fe0 mass concentrations (g/L) to obtain ksa presented in Figure 3.
(2)
11 ACS Paragon Plus Environment
Environmental Science & Technology
Page 12 of 24
324
As seen in Figure 3, the ksa for S-nZVIco showed a rapid increase from 0.61×10-3 to 23.06×10-3 L m-2 h-1
325
between [S/Fe]dosed of 0.035 and 0.4, respectively. The increase in rate constants can be attributed to the
326
increasing association of FeS and Fe0 with increasing [S/Fe]dosed. Electron conduction by iron oxides and iron
327
polysulfides deposited on nZVI is less efficient compared to electron conduction by FeS
328
the rapid increase in TCE degradation rate constants observed for S-nZVIco, the contribution of iron oxides
329
and iron polysulfides to the overall ksa is likely negligible. FeS has also been reported to be more water-
330
wetting (less hydrophobic) compared to iron oxides 28 and thus, the observed rate constants are unlikely to be
331
an effect of increased sorption of TCE to FeS. The rapid rise in the ksa from 0.2 to 0.4 is likely related to the
332
increase in the FeS structures embedded in and present around the particles (Figure 1a) that substantially
333
improve electron conduction to TCE molecules at the surface. The ksa for Pd-nZVI with 0.5 wt.% Pd in
334
Figure 3, was 1.43×10-3 L m-2 h-1 which was comparable to degradation rates of S-nZVIco between [S/Fe]dosed
335
of 0.05 and 0.1. By increasing the Pd content to 2.5% and 5%, we observed a linear increase in the ksa with it
336
being 16×10-3 L m-2 h-1 at 5 wt.% Pd (Figure S6). This suggests that under Fe0 limited conditions, the ksa was
337
limited by the number of Pd sites.33 Thus, in order to achieve rate constants comparable to S-nZVIco at
338
[S/Fe]dosed greater than 0.1, higher loadings of Pd are needed on nZVI which can significantly add to the
339
costs of remediation.
340
The ksa for S-nZVIpost and S-nZVIco were similar between [S/Fe]dosed of 0.035 and 0.1. However between
341
[S/Fe]dosed of 0.1 and 0.4, the ksa of S-nZVIpost decreased from 1.03×10-3 to 0.26×10-3 L m-2 h-1. This decrease
342
in degradation rates was likely due to increased oxide growth near the particle surface (discussed in the
343
section below). Because the location of FeS is at the particle surface in S-nZVIpost, the growth of more
344
oxides at the surface likely slows down the efficiency of electron conduction, thereby retarding the
345
degradation kinetics. Additionally between [S/Fe]dosed of 0.1 and 0.4, a significant amount of HS- remained
346
dissolved in the aqueous suspension (Figure 2b), which may have also contributed to the slowing down of
347
TCE degradation rate.11
348
We also evaluated the performance of the nanoparticles under Fe0 excess conditions. As seen in Figure S7,
349
the ksa values for S-nZVIco increased from 0.34×10-3 L m-2 h-1 at [S/Fe]dosed of 0.035, to 3.46×10-3 L m-2 h-1 at
350
[S/Fe]dosed of 0.2 and did not change thereafter likely due to the attainment of optimal number of FeS binding
351
sites for the limited mass of TCE employed. S-nZVIpost displayed an optimum ksa of 1.98×10-3 L m-2 h-1 at
352
[S/Fe]dosed of 0.1. Pd-nZVI (0.5 wt.% Pd) had a ksa of 79.61 ×10-3 L m-2 h-1 which was 56 times higher than
353
that under Fe0 limited conditions. Under Fe0 excess conditions, the rapid reaction kinetics of Pd-nZVI with
354
water to produce hydrogen (shown in Figure 4) likely resulted in rapid hydrogenation of TCE and high
355
dechlorination rate.
29, 31, 32
, and given
12 ACS Paragon Plus Environment
Page 13 of 24
Environmental Science & Technology
356
S-nZVIco does not produce H2 during TCE degradation but its reactivity to pure water is higher than
357
S-nZVIpost. An important observation from the reactivity studies under Fe0 limited conditions was the
358
absence of hydrogen generation during TCE degradation reactions, for S-nZVIco, S-nZVIpost and Pd-nZVI.
359
Hydrogen is produced by the corrosion of Fe0 by water and amendment of nZVI with Pd or S can influence
360
its reactivity to water. Previous studies investigating the hydrogen generation rate of S-nZVI particles
361
(synthesized using the two-step approach) reported the suppression of reaction rates with water.15,
362
Therefore we conducted separate kinetic experiments with nZVI, Pd-nZVI, S-nZVIco and S-nZVIpost to
363
evaluate their hydrogen generation ability in pure water in the absence of TCE (Figure S8).
364
As shown in Figure S8, H2 evolution profiles of S-nZVIco and S-nZVIpost followed zero order kinetics.
365
However we observed that Pd-nZVI and nZVI showed deviations from the zero order kinetics after 24 h and
366
60 h respectively. Pd-nZVI particles generated large amounts of H2 within 24 hrs and likely deviated from
367
zero order kinetics due to rapid depletion of Fe0 as it reached the stoichiometric maximum. In the case of
368
nZVI particles, the deviation from zero order kinetics was likely due to the effect of progressively thickening
369
surface oxides which slowed down electron conduction. Therefore, in order to draw a comparison with the
370
zero-order kinetics displayed by S-nZVIpost and S-nZVIco, we used the initial zero-order rate constants for
371
Pd-nZVI (estimated from time points up to 24 h) and nZVI (estimated from time points up to 60 h). Their
372
surface area normalized rate constants (9:; ) were computed by normalizing the observed rate constants with
373
BET surface areas and Fe0 mass concentrations and are presented in Figure 4.
374
As seen in Figure 4, the 9:; for nZVI was 0.054 µmoles L m-2 h-1 while at [S/Fe]dosed of 0.035, the 9:; for S-
375
nZVIco was 0.035 µmoles L m-2 h-1. A possible explanation for the higher 9:; of nZVI compared to S-
376
nZVIco is the higher affinity of Fe-oxides than FeS, to water.15 However by increasing the [S/Fe]dosed, the
377
number of electron conduction sites in S-nZVIco increase due to higher amounts of FeS, which increases the
378
9:; to 0.071 µmoles L m-2 h-1 at [S/Fe]dosed of 0.4. Similar to reactivity with TCE, S-nZVIpost displayed a
379
lower 9:; (0.019 to 0.023 µmoles L m-2 h-1) compared to S-nZVIco. This was likely due to lower amounts of
380
FeS (Figure 2c) and lower accessibility of electrons due to the FeS distribution pattern (Figure 1b).
381
Overall, H2 generation rates of S-nZVIpost in contact with pure water was lower than nZVI, in the range of
382
[S/Fe]dosed investigated. This is in good agreement with prior studies.15,
383
comparable or slightly higher H2 generation rates than nZVI, at higher [S/Fe]dosed.
384
Morphology of S-nZVIco after reaction with TCE: The oxidized nanoparticles were retrieved after their
385
reaction with TCE, in order to characterize changes in their surface chemistry and morphology. The
386
morphological changes are shown in TEM images in Figures 5a and 5b. As seen in the figures, the particles
387
looked significantly different at the end of their reaction lifetime. For the oxidized S-nZVIco (Figure 5a) the
21
21, 22
In contrast, S-nZVIco showed
13 ACS Paragon Plus Environment
Environmental Science & Technology
Page 14 of 24
388
plate like precipitates, provided high O signals alongwith Fe and S in the EDS analysis, suggesting that they
389
were a mixture of iron oxides and sulfides (Figure S9 a). XPS spectra (Figure S9 c and d) revealed the
390
presence of higher amounts of polysulfide species after reaction with TCE compared to unreacted S-nZVIco.
391
The scattered distribution of the precipitates for S-nZVIco suggests the outgrowth of oxides away from the
392
particle surface. In the case of S-nZVIpost (Figure 5b), spherical shapes were discernible along with some
393
hollowed out particles which are attributable to the Kirkendall effect.11 The nanoparticle surfaces appeared
394
to be covered with a thick mesh of needle like structures which were a mix of iron oxides and sulfides
395
(Figure S9 b). It is likely that the presence of FeS structures at the surface of S-nZVIpost behaved as a surface
396
coating which caused restricted outgrowths of the oxides. XPS analysis revealed peaks corresponding to FeS
397
and polysulfides (Figure S9 e and f). The Pd-nZVI particles also had outgrowth of oxides in the absence of
398
any restricting surface coatings as shown in our previous study.24
399
Implications
400
To our knowledge, this is the first study that demonstrates S-nZVI reactivity with TCE comparable to Pd-
401
nZVI under Fe0 limited conditions. Fe0 limited (TCE excess) conditions can be expected at source zones
402
where TCE NAPL is present. Although the mechanism of TCE degradation facilitated by Pd0 is different
403
from FeS, the results from this study highlight that in composite nanoparticles, structural attributes can play
404
as significant a role in enhancing reactivity, as chemical composition. In scenarios where contaminant mass
405
is low (Fe0 excess), Pd-nZVI exhibits high TCE dechlorination rates. However Pd-nZVI also undergoes
406
rapid reactions with water to produce hydrogen, which consumes Fe0. This may add considerably to
407
treatment costs in field operations wherein the poorly mixed subsurface conditions can result in rapid loss of
408
Pd-nZVI reductive capacity through reactions with water without efficiently treating the contaminant. This
409
may lead to requirement of frequent re-injections of Pd-nZVI suspensions resulting in undesirable
410
consequences such as decreased aquifer porosity. Conversely, S-nZVIco exhibits lower reactivity to water
411
and higher selectivity to TCE which may make it more suitable for field applications. They are also more
412
reactive than S-nZVIpost.
413
Prior studies have demonstrated that sulfidation of nZVI enables degradation of other recalcitrant chlorinated
414
contaminants such as 1,2 DCA over extended periods of time17. Thus, further research investigating the
415
effectiveness of S-nZVIco in treating other challenging chlorinated ethenes and ethanes are required to better
416
understand its reactivity potential.
417
For in situ remediation there are other important considerations beyond reactivity. For example, effective
418
injection and transport of nanoparticles in the sub-surface requires that they be colloidally stable. S-nZVIco
419
has higher surface charge and lower aggregate sizes compared to nZVI suggesting that it has good transport
14 ACS Paragon Plus Environment
Page 15 of 24
Environmental Science & Technology
420
potential. Our recent studies show that dissolved organic matter at environmentally relevant concentrations is
421
unlikely to influence the reactivity of S-nZVI.34 Furthermore, previous studies demonstrated that
422
groundwater composition only has a limited effect on the reactivity of S-nZVI.15, 35 A cost analysis based on
423
prices of reagents (high purity chemicals) shows that at comparable dechlorination rates and extents, the cost
424
of degradation of a unit mass of TCE using Pd-nZVI is 70% higher than that using S-nZVIco (Table S8).
425
Thus, S-nZVIco appear to be cost–effective agents for TCE degradation, particularly for source zones.
426
Supporting Information Available
427
TEM-EDS and XPS of S-nZVIco and S-nZVIpost before and after reaction with TCE; BET surface areas; TCE
428
degradation profiles; TCE degradation end product quantification; electron balance calculations; hydrogen
429
evolution profiles. This information is available free of charge via the Internet at http://pubs.acs.org.
430
Acknowledgement
431
The research was funded by the Natural Sciences and Engineering Research Council of Canada (Grant
432
Numbers RGPIN-2016-05022, RGPAS-492998-16, I2IPJ-501965-16). We thank Josianne Lefebvre
433
(Polytechnique Montreal) and David Liu (McGill) for assistance with XPS and TEM-EDS analyses,
434
respectively.
435 436 437 438 439
References
440 441 442 443 444 445 446 447 448 449 450 451 452
1. Mukherjee, R.; Kumar, R.; Sinha, A.; Lama, Y.; Saha, A. K., A review on synthesis, characterization, and applications of nano zero valent iron (nZVI) for environmental remediation. Critical Reviews in Environmental Science and Technology 2016, 46, (5), 443-466. 2. O’Carroll, D.; Sleep, B.; Krol, M.; Boparai, H.; Kocur, C., Nanoscale zero valent iron and bimetallic particles for contaminated site remediation. Advances in Water Resources 2013, 51, 104-122. 3. Fan, D.; O'Carroll, D. M.; Elliott, D. W.; Xiong, Z.; Tratnyek, P. G.; Johnson, R. L.; Garcia, A. N., Selectivity of nano zerovalent iron in in situ chemical reduction: Challenges and improvements. Remediation Journal 2016, 26, (4), 27-40. 4. Schöftner, P.; Waldner, G.; Lottermoser, W.; Stöger-Pollach, M.; Freitag, P.; Reichenauer, T. G., Electron efficiency of nZVI does not change with variation of environmental parameters. Science of The Total Environment 2015, 535, 69-78. 5. Mackenzie, K.; Bleyl, S.; Georgi, A.; Kopinke, F.-D., Carbo-Iron–An Fe/AC composite–As alternative to nano-iron for groundwater treatment. Water research 2012, 46, (12), 3817-3826. 15 ACS Paragon Plus Environment
Environmental Science & Technology
453 454 455 456 457 458 459 460 461 462 463 464 465 466 467 468 469 470 471 472 473 474 475 476 477 478 479 480 481 482 483 484 485 486 487 488 489 490 491 492 493 494 495 496 497 498 499 500
Page 16 of 24
6. Lien, H.-L.; Zhang, W.-x., Nanoscale iron particles for complete reduction of chlorinated ethenes. Colloids and Surfaces A: Physicochemical and Engineering Aspects 2001, 191, (1-2), 97-105. 7. Sakulchaicharoen, N.; O'Carroll, D. M.; Herrera, J. E., Enhanced stability and dechlorination activity of pre-synthesis stabilized nanoscale FePd particles. Journal of contaminant hydrology 2010, 118, (3-4), 117-127. 8. EU, Water Framework Directive 2000/60/EC. 9. Pearce, C. I.; Pattrick, R. A.; Vaughan, D. J., Electrical and magnetic properties of sulfides. Reviews in Mineralogy and Geochemistry 2006, 61, (1), 127-180. 10. Fan, D.; Lan, Y.; Tratnyek, P. G.; Johnson, R. L.; Filip, J.; O’Carroll, D. M.; Nunez Garcia, A.; Agrawal, A., Sulfidation of iron-based materials: A review of processes and implications for water treatment and remediation. Environmental Science & Technology 2017, 51, (22), 13070-13085. 11. Fan, D.; Anitori, R. P.; Tebo, B. M.; Tratnyek, P. G.; Lezama Pacheco, J. S.; Kukkadapu, R. K.; Engelhard, M. H.; Bowden, M. E.; Kovarik, L.; Arey, B. W., Reductive sequestration of pertechnetate (99TcO4–) by nano zerovalent iron (nZVI) transformed by abiotic sulfide. Environmental science & technology 2013, 47, (10), 5302-5310. 12. Su, Y.; Adeleye, A. S.; Keller, A. A.; Huang, Y.; Dai, C.; Zhou, X.; Zhang, Y., Magnetic sulfide-modified nanoscale zerovalent iron (S-nZVI) for dissolved metal ion removal. Water research 2015, 74, 47-57. 13. Song, S.; Su, Y.; Adeleye, A. S.; Zhang, Y.; Zhou, X., Optimal design and characterization of sulfidemodified nanoscale zerovalent iron for diclofenac removal. Applied Catalysis B: Environmental 2017, 201, 211-220. 14. Cao, Z.; Liu, X.; Xu, J.; Zhang, J.; Yang, Y.; Zhou, J.; Xu, X.; Lowry, G. V., Removal of antibiotic florfenicol by sulfide-modified nanoscale zero-valent iron. Environmental science & technology 2017, 51, (19), 11269-11277. 15. Rajajayavel, S. R. C.; Ghoshal, S., Enhanced reductive dechlorination of trichloroethylene by sulfidated nanoscale zerovalent iron. Water research 2015, 78, 144-153. 16. Kim, E.-J.; Kim, J.-H.; Azad, A.-M.; Chang, Y.-S., Facile synthesis and characterization of Fe/FeS nanoparticles for environmental applications. ACS applied materials & interfaces 2011, 3, (5), 1457-1462. 17. Nunez Garcia, A.; Boparai, H. K.; O’Carroll, D. M., Enhanced dechlorination of 1, 2-dichloroethane by coupled nano iron-dithionite treatment. Environmental science & technology 2016, 50, (10), 5243-5251. 18. Li, D.; Mao, Z.; Zhong, Y.; Huang, W.; Wu, Y.; Peng, P. a., Reductive transformation of tetrabromobisphenol A by sulfidated nano zerovalent iron. Water research 2016, 103, 1-9. 19. Ma, X.; He, D.; Jones, A. M.; Collins, R. N.; Waite, T. D., Reductive reactivity of borohydride-and dithionite-synthesized iron-based nanoparticles: A comparative study. Journal of hazardous materials 2016, 303, 101-110. 20. Su, Y.; Adeleye, A. S.; Huang, Y.; Zhou, X.; Keller, A. A.; Zhang, Y., Direct synthesis of novel and reactive sulfide-modified nano iron through nanoparticle seeding for improved cadmium-contaminated water treatment. Scientific reports 2016, 6, 24358. 21. Han, Y.; Yan, W., Reductive Dechlorination of Trichloroethene by Zero-valent Iron Nanoparticles: Reactivity Enhancement through Sulfidation Treatment. Environmental science & technology 2016, 50, (23), 12992-13001. 22. Fan, D.; O’Brien Johnson, G.; Tratnyek, P. G.; Johnson, R. L., Sulfidation of nano zerovalent iron (nZVI) for improved selectivity during in-situ chemical reduction (ISCR). Environmental science & technology 2016, 50, (17), 9558-9565. 23. Li, J.; Zhang, X.; Sun, Y.; Liang, L.; Pan, B.; Zhang, W.; Guan, X., Advances in Sulfidation of Zerovalent Iron for Water Decontamination. Environmental science & technology 2017, 51, (23), 13533-13544. 24. Bhattacharjee, S.; Ghoshal, S., Phase transfer of palladized nanoscale zerovalent iron for environmental remediation of trichloroethene. Environmental science & technology 2016, 50, (16), 86318639. 16 ACS Paragon Plus Environment
Page 17 of 24
501 502 503 504 505 506 507 508 509 510 511 512 513 514 515 516 517 518 519 520 521 522 523 524 525 526 527 528 529 530
Environmental Science & Technology
25. Liu, Y.; Majetich, S. A.; Tilton, R. D.; Sholl, D. S.; Lowry, G. V., TCE dechlorination rates, pathways, and efficiency of nanoscale iron particles with different properties. Environmental science & technology 2005, 39, (5), 1338-1345. 26. Fatisson, J.; Ghoshal, S.; Tufenkji, N., Deposition of carboxymethylcellulose-coated zero-valent iron nanoparticles onto silica: roles of solution chemistry and organic molecules. Langmuir 2010, 26, (15), 12832-12840. 27. Shi, X.; Sun, K.; Balogh, L. P.; Baker Jr, J. R., Synthesis, characterization, and manipulation of dendrimer-stabilized iron sulfide nanoparticles. Nanotechnology 2006, 17, (18), 4554. 28. Zhang, Y.; Zhi, Y.; Liu, J.; Ghoshal, S., Sorption of Perfluoroalkyl Acids to Fresh and Aged Nanoscale Zerovalent Iron Particles. Environmental science & technology 2018, 52, (11), 6300-6308. 29. Gu, Y.; Wang, B.; He, F.; Bradley, M. J.; Tratnyek, P. G., Mechanochemically sulfidated microscale zero valent iron: Pathways, kinetics, mechanism, and efficiency of trichloroethylene dechlorination. Environmental Science & Technology 2017, 51, (21), 12653-12662. 30. Nurmi, J. T.; Tratnyek, P. G.; Sarathy, V.; Baer, D. R.; Amonette, J. E.; Pecher, K.; Wang, C.; Linehan, J. C.; Matson, D. W.; Penn, R. L., Characterization and properties of metallic iron nanoparticles: spectroscopy, electrochemistry, and kinetics. Environmental Science & Technology 2005, 39, (5), 12211230. 31. Lee, W.; Batchelor, B., Abiotic reductive dechlorination of chlorinated ethylenes by iron-bearing soil minerals. 1. Pyrite and magnetite. Environmental Science & Technology 2002, 36, (23), 5147-5154. 32. Butler, E. C.; Hayes, K. F., Kinetics of the transformation of trichloroethylene and tetrachloroethylene by iron sulfide. Environmental Science & Technology 1999, 33, (12), 2021-2027. 33. Xie, Y.; Cwiertny, D. M., Chlorinated solvent transformation by palladized zerovalent iron: Mechanistic insights from reductant loading studies and solvent kinetic isotope effects. Environmental science & technology 2013, 47, (14), 7940-7948. 34. Bhattacharjee, S.; Ghoshal, S., Sulfidation of nanoscale zerovalent iron in the presence of two organic macromolecules and its effects on trichloroethene degradation. Environmental Science: Nano 2018, 5, (3), 782-791. 35. Kim, E.-J.; Murugesan, K.; Kim, J.-H.; Tratnyek, P. G.; Chang, Y.-S., Remediation of trichloroethylene by FeS-coated iron nanoparticles in simulated and real groundwater: effects of water chemistry. Industrial & Engineering Chemistry Research 2013, 52, (27), 9343-9350.
531 532
17 ACS Paragon Plus Environment
Environmental Science & Technology
Page 18 of 24
533
List of Figures
534
Figure 1: (a) representative TEM image of S-nZVIco - (a1)-(a4) are blown-up images of the sections
535
highlighted by the dotted boxes in Figure 1a; (b) representative TEM image of S-nZVIpost – (b1) is the
536
blown-up image of the dotted boxed area in Figure 1b.
537
Figure 2: (a) Specific degradation capacities (SDC) of S-nZVIco, S-nZVIpost and Pd-nZVI particles; inset
538
images represent conceptualized schematics for the different nanoparticles (b) TCE degradation end product
539
distribution for Pd-nZVI, S-nZVIco and S-nZVIpost ([S/Fe]dosed = 0.4) (c) [S/Fe]particle for S-nZVIco (inset
540
figure) and S-nZVIpost; undeposited sulfur was measured in the aqueous phase and accounted for >97% mass
541
balance (d) Specific degradation capacities plotted as a function of [S/Fe]particle. Lines are drawn to guide the
542
eye and error bars represent standard deviation from triplicate reactors.
543
Figure 3: Surface area normalized pseudo first order TCE degradation rate constants (ksa) at different
544
[S/Fe]dosed under Fe0 limited conditions. Error bars represent standard deviation from triplicate reactors.
545
Figure 4: Surface area normalized zero order hydrogen evolution rate constants for nZVI, S-nZVIco, S-
546
nZVIpost and Pd-nZVI. Error bars represent standard deviation from triplicate reactors.
547
Figure 5: TEM image of (a) S-nZVIco and (d) S-nZVIpost , after reaction with TCE ([S/Fe]dosed = 0.4).
548 549
18 ACS Paragon Plus Environment
Page 19 of 24
550
Environmental Science & Technology
Figure 1
(a)
Type I
(a1)
Type I
(a2)
Type II
(a3)
Type III
(a4)
a3 a1
a2
a4
551
(b1)
(b)
Type IV b1
0.5 µm
552 553
Type I
554 555 556 557
19 ACS Paragon Plus Environment
Environmental Science & Technology
0.6
(a)
% product formed
0.5 0.4 0.3 0.2 S-nZVI co S-nZVI post
0.1
Pd-nZVI 0.0
(moles of each product /moles of total products)
Figure 2
Specific Degradation Capacity 0 (moles of TCE degraded/mole of Fe )
558
Page 20 of 24
(b)
100
Ethene Acetylene Ethane 1-butene trans-2-butene cis- 2-butene 1,1-DCE cis 1,2 DCE Other
80 60 40 20 0
-0.1 Pd-nZVI
0.0
0.1
0.2
0.3
0.4
Pd-nZVI
0.5
S-nZVI co
S-nZVI post
0.06 (c)
S-nZVIpost
0.04
0.4
[S/Fe]particle
[S/Fe]particle
0.05
0.03 0.02
0.3 0.2 0.1 0.0 0.0
0.01
S-nZVIco 0.1
0.2
0.3
0.4
[S/Fe]dosed
0.00 0.0
0.1
0.2
0.3
0.4
0.5
Specific Degradation Capacity 0 (moles of TCE degraded/mole of Fe )
[S/Fe]dosed
0.6 (d) 0.5 0.4 0.3 0.2 S-nZVI co S-nZVI post
0.1
Pd-nZVI 0.0 -0.1 0.0 Pd-nZVI
[S/Fe]dosed
0.1
0.2
0.3
0.4
0.5
[S/Fe]particle
559 560 561
20 ACS Paragon Plus Environment
Page 21 of 24
562
Environmental Science & Technology
Figure 3
25 S-nZVIco S-nZVIpost Pd-nZVI
3
k sa (L m -2 h -1) x 10 -3
k sa
20
2 1
15
0 Pd-nZVI -0.1 0.0
0.1 0.2 0.3 0.4
[S/Fe]dosed
10
5
0 -0.1 Pd-nZVI 563
0.0
0.1
0.2
0.3
0.4
0.5
[S/Fe]dosed
564
21 ACS Paragon Plus Environment
Environmental Science & Technology
565
Page 22 of 24
Figure 4
20.00 nZVI S-nZVIco S-nZVIpost Pd-nZVI
-2
-1
k H 2 (µmoles L m h )
18.00
0.08 0.06 0.04 0.02 0.00 -0.1 Pd-nZVI
566
0.0
0.1
0.2
0.3
0.4
0.5
[S/Fe]dosed
567
22 ACS Paragon Plus Environment
Page 23 of 24
568
Environmental Science & Technology
Figure 5 (a)
(b)
569 570
23 ACS Paragon Plus Environment
Environmental Science & Technology
571
Page 24 of 24
TOC
572
24 ACS Paragon Plus Environment