Photoluminescence Lifetimes and Thermal Degradation of Mn2+-

Sep 21, 2018 - The Mn2+ doped CsPbCl3 nanocrystals (NCs) with low Mn2+ doping concentration were synthesized using different reaction temperature to ...
0 downloads 0 Views 1MB Size
Subscriber access provided by University of South Dakota

C: Physical Processes in Nanomaterials and Nanostructures

Photoluminescence Lifetimes and Thermal Degradation of Mn -Doped CsPbCl Perovskite Nanocrystals 2+

3

Sihang Ji, Xi Yuan, Ji Li, Jie Hua, Yunjun Wang, Ruosheng Zeng, Haibo Li, and Jialong Zhao J. Phys. Chem. C, Just Accepted Manuscript • Publication Date (Web): 21 Sep 2018 Downloaded from http://pubs.acs.org on September 21, 2018

Just Accepted “Just Accepted” manuscripts have been peer-reviewed and accepted for publication. They are posted online prior to technical editing, formatting for publication and author proofing. The American Chemical Society provides “Just Accepted” as a service to the research community to expedite the dissemination of scientific material as soon as possible after acceptance. “Just Accepted” manuscripts appear in full in PDF format accompanied by an HTML abstract. “Just Accepted” manuscripts have been fully peer reviewed, but should not be considered the official version of record. They are citable by the Digital Object Identifier (DOI®). “Just Accepted” is an optional service offered to authors. Therefore, the “Just Accepted” Web site may not include all articles that will be published in the journal. After a manuscript is technically edited and formatted, it will be removed from the “Just Accepted” Web site and published as an ASAP article. Note that technical editing may introduce minor changes to the manuscript text and/or graphics which could affect content, and all legal disclaimers and ethical guidelines that apply to the journal pertain. ACS cannot be held responsible for errors or consequences arising from the use of information contained in these “Just Accepted” manuscripts.

is published by the American Chemical Society. 1155 Sixteenth Street N.W., Washington, DC 20036 Published by American Chemical Society. Copyright © American Chemical Society. However, no copyright claim is made to original U.S. Government works, or works produced by employees of any Commonwealth realm Crown government in the course of their duties.

Page 1 of 26 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

The Journal of Physical Chemistry

Photoluminescence Lifetimes and Thermal Degradation of Mn2+-Doped CsPbCl3 Perovskite Nanocrystals ‡

Sihang Ji,† Xi Yuan,*,† Ji Li,† Jie Hua,† Yunjun Wang, Ruosheng Zeng,§ Haibo Li† and Jialong Zhao*,† †

Key Laboratory of Functional Materials Physics and Chemistry of the Ministry of

Education, Jilin Normal University, Siping 136000, China ‡

§

Suzhou Xingshuo Nanotech Co., Ltd. (Mesolight), Suzhou 215123, China School of Life and Environmental Sciences, Guilin University of Electronic

Technology, Guilin 541004, China

1

ACS Paragon Plus Environment

The Journal of Physical Chemistry 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 2 of 26

ABSTRACT The Mn2+ doped CsPbCl3 nanocrystals (NCs) with low Mn2+ doping concentration were synthesized using different reaction temperature to control the NC size from 5.3 nm to 17.4 nm and then were studied by means of steady-state and time-resolved photoluminescence (PL) spectroscopy at various temperatures. The Mn2+ emissions with different quantum yields in the doped NCs in hexane exhibited nearly size-independent and single-exponentially decayed lifetimes of 1.8 ms at room temperature. The PL lifetimes in all Mn2+ in CsPbCl3 doped NCs had similar temperature dependence from 80 to 300 K while they were size-dependent at elevated temperatures, reflecting thermal degradation of doped NCs. The degradation mechanisms of Mn2+ PL were attributed to amount of surface defects as nonradiative recombination centers generated in size-unchanged and grown Mn2+:CsPbCl3 NCs. The study provides the detailed understanding of the thermal degradation mechanisms in doped perovskite NCs for optoelectronic applications.

2

ACS Paragon Plus Environment

Page 3 of 26 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

The Journal of Physical Chemistry

1. INTRODUCTION All-inorganic halide perovskite nanocrystals (NCs) have been paid much attention due to their size- or composition-tunable photoluminescence (PL) wavelength, high PL quantum yield (QY), and narrow emission linewidth, which exhibit the practical applications in solar cells, photodetectors, and light emitting diodes.1-3 Highly luminescent manganese ion (Mn2+) doped CsPbCl3 perovskite NCs with a bright orange Mn2+ emission band around 600 nm were successfully synthesized in 2016.4-20 It is well known that the broad orange-red emissions of Mn2+ doped in traditional II-VI semiconductor NCs are attributed to the Mn2+ 4T1→6A1 d−d transition through energy transfer from excitons in the host to dopants, which can be used for white light emitting devices.21-30 The most commonly studied Mn2+ emissions are usually observed at around 2.12 eV (585 nm) from Mn2+ doped ZnS and ZnSe NCs while they are at 2.06 eV (600 nm) for Mn2+ in CdS and CdSe NCs.21,26-30 The tunable Mn2+ emissions from yellow to red were observed in Mn2+ doped NCs with varying not only the concentrations and positions of dopants but also the sizes and structures of NCs.31-37 At the same time, the various PL lifetimes of Mn2+ emissions were reported from microseconds to milliseconds because the spin-forbidden Mn2+ d−d transitions in doped II-VI semiconductor NCs were influenced by spin-orbit coupling at the Mn2+ and the anion.38-43 Therefore, tuning the energies of Mn2+ emissions in CsPbCl3 NCs is promising to achieve novel functionalities and superior advantages for white light emitting diodes by changing the NC composition and size and the dopant concentration. 3

ACS Paragon Plus Environment

The Journal of Physical Chemistry 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 4 of 26

Recently, the emitting colors of Mn2+ doped CsPbCl3 NCs have been controlled for fabrication of the warm white light emitting diodes. The wavelength of exciton emission in CsPbCl3 were tuned to 450 nm through anion exchange of Mn:CsPbCl3 NCs with PbBr2 to obtain Mn:CsPbClxBr3−x NCs.4,19 Meantime the emission wavelength of Mn2+ in CsPbCl3 NCs was shifted from 595 nm to 620 nm by changing the Mn2+ doping concentration from low to high while the PL dynamics was significantly reduced from a single-exponential decay lifetime of 1.6 ms to multi-exponential decay one of about 0.4 ms at room temperature,5-11 which is attributed to formation of Mn2+-Mn2+ dimers or defects at higher Mn2+ doping level.15,18 However, the NC size dependence of the PL energy and lifetime for Mn2+ doped in CsPbCl3 NCs has not been reported yet. Further improving the stability of CsPbX3 NCs by doping Mn2+ in the host has been demonstrated recently.14 Therefore it is convenient to reveal thermal stability of Mn2+ in Mn:CsPbCl3 NCs by monitoring the change in their single-exponentially decayed PL lifetimes, which is very important for the practical applications in solid state lighting. In this work, the size-varied Mn2+:CsPbCl3 NCs with low doping concentration were synthesized using different reaction temperature and then studied by variable-temperature steady-state and time-resolved PL spectroscopy. It is surprisingly found that the Mn2+ emissions with different QYs in all the doped NCs in hexane almost exhibit the same single-exponentially decayed time of 1.8 ms at room temperature and the same temperature dependence of lifetimes from 80 to 300 K. The thermal degradation mechanisms of Mn2+ emissions in doped NCs with varied size 4

ACS Paragon Plus Environment

Page 5 of 26 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

The Journal of Physical Chemistry

were studied in vacuum at temperature ranging from 300 to 400 K by measuring the change in PL intensity, lifetime, NC size, and structure.

2. EXPERIMENTAL SECTION Materials. MnCl2 (≥99%), PbCl2 (99.99%), Cs2CO3 (99.99%), and trioctylphosphine (TOP, 90%) were purchased from Aladdin. Oleylamine (OLA, 70%) and oleic acid (OA, 90%) were purchased from Aldrich. 1-Octadecene (ODE, 90%,) was purchased from Alfa Aesar. Hexane, toluene, acetone, and ethanol were purchased from Beijing Chemical Works. All chemicals were directly used without further purification. Synthesis of Cs-oleate precursor. The Cs2CO3 of 0.26 g, ODE of 7 mL, and OA of 1 mL were loaded into the three necked flask, then degassed at 120 °C for 30 min. After that, the mixed solution was heated up to 150 °C under the protection of argon, and held at least 15 min until the solution became clear and transparent. Synthesis of Mn:CsPbCl3 NCs. The Mn2+:CsPbCl3 NCs with varied particle sizes were synthesized using a one-pot injection synthesis method, which was modified from previously reported approaches. In a typical procedure, the PbCl2 (0.2 mmol, 0.054 g), and MnCl2 (0.4 mmol, 0.05 g) were mixed with OLA (1.5 mL), OA (1.5 mL), TOP (1 mL), and ODE (6 mL) in a 50 mL three necked flask. The reaction mixture was degassed at 120 °C for 30 min, and then heated up to 190 °C under argon flow. 0.25 mL of Cs-oleate precursor (made by dissolving Cs2CO3, 0.26 g, in OA, 1 mL, and ODE, 7 mL, at 150 °C) was quickly injected into the reaction solution, and after 15 s the solution was immediately cooled down to room temperature by 5

ACS Paragon Plus Environment

The Journal of Physical Chemistry 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 6 of 26

immersion in a cold-water bath. The Mn2+:CsPbCl3 NCs with different particle sizes could be obtained by varying reaction temperature, surface ligand content and reaction solution concentration. Keeping the other conditions constant, when the reactants of 130 °C are injected into the precursor, the small size about 5.3 nm NCs were synthesized. Large NCs with about 17.4 nm were synthesized at 210 °C by adding appropriate ligands and reaction solvents. For purification, the Mn2+:CsPbCl3 NCs were repeatedly precipitated by acetone/hexane, centrifuged, decanted, and suspended in hexane. The final precipitates were dispersed in hexane. The Mn2+ doping concentrations of Mn:CsPCl3 NCs with various sizes were measured to be 3.0%, 3.1%, 2.9%, 2.8%, and 2.7%, respectively, for NC397, 400, 403, 406, and 409 by inductively coupled plasma-mass spectrometer (ICP-MS). Characterization.

Absorption

spectra

were

recorded

on

a

UV-visible

spectrophotometer (Shimadzu UV-2700). PL and 2D PL excitation spectra, PL QYs, and PL decay curves were carried out by using a spectrometer (Horiba Jobin Yvon Fluorolog-3) with a QY accessory and a time-correlated single-photon counting lifetime spectroscopy system. The morphologies of the NCs were acquired by using a JEOL JEM2100 TEM. XRD patterns were measured by a Rigaku D/max-2500 diffractometer using Cu Kα radiation. A PerkinElmer Nexion 350-X ICP-MS was used for elemental analysis. A Janis VPF-500 vacuum liquid nitrogen cryostat with a temperature controller was used to mount the Mn2+:CsPbCl3 NC film samples (on silicon substrates) for the temperature dependent PL measurements.

6

ACS Paragon Plus Environment

Page 7 of 26 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

The Journal of Physical Chemistry

3. RESULTS AND DISCUSSION

Figure 1. Absorption (a), PL (b), PL excitation spectra (c), Mn2+ PL decay curves (d), PL lifetimes and QYs (e) of Mn2+:CsPbCl3 NCs with varied sizes. The color in (c) represents the intensity of the emission bands. All NCs are dispersed in hexane solutions.

Following the methods adapted from the literature,4,5,15 Mn2+:CsPbCl3 NCs with selected five sizes were synthesized by changing the reaction temperature. The detailed synthesis procedure is provided in Experimental Section. Figure 1 shows the absorption, PL, and PL excitation (PLE) spectra, Mn2+ PL decay curves, PL lifetimes, and PL QYs of differently sized Mn2+:CsPbCl3 NCs. As seen in Figure 1a and b, the absorption spectra show well-resolved peaks from exciton states in Mn2+:CsPbCl3 NCs synthesized at various reaction temperatures. The sharp lowest exciton absorption bands of these NCs shift to the high energy side from 402 nm to 386 nm with decreasing the NC size, indicating the quantum size effect. The blue shift of exciton absorption band is only 130 meV. It is known that the size of as-prepared NCs is much larger than their exciton Bohr radius (2.5 nm) of CsPbCl3, so that the 7

ACS Paragon Plus Environment

The Journal of Physical Chemistry 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 8 of 26

quantum size effect is not significant.44 The double emission bands peaked at around 400 nm and 598 nm are clearly observed from each Mn2+:CsPbCl3 NCs in Figure 1b, which are considered to originate from the radiative recombination of excitons near the band edge and the isolated Mn2+ ions, respectively.4,5 The wavelengths of exciton luminescence bands are 397, 400, 403, 406, and 409 nm, thus the NC samples are labeled as NC397, 400, 403, 406, and 409, respectively. In addition, it is noted that the full width at the half maximum (FWHM) of exciton emission in Mn2+:CsPbCl3 NCs slightly increases with decreasing the NC size. However, it is surprisingly observed that the Mn2+ luminescence band keeps a constant peak wavelength at 598 nm for all the differently sized Mn2+:CsPbCl3 NCs.5 In addition, no clear change in the FWHMs of NCs is also observed. On the other hand, the PL wavelengths of excitons and Mn2+ keep unchanged when the PL excitation wavelength is varied from 280 to 385 nm as seen in Figure 1c, indicating relatively uniform size distribution.45 It is interesting that all the Mn2+:CsPbCl3 NCs with different size exhibit almost the same Mn2+ PL decay curves as seen in Figure 1d. This means that the NC size has no effect on their PL lifetimes, which is quite different from those of Mn2+ doped ZnS and ZnSe NCs in the previous reports.38-43 The PL decay curves were well fitted by a single exponential function I(t)=I0×exp(-t/τ), where I0 and τ are the initial intensity and time constant. The PL lifetimes of Mn2+ in CsPbCl3 NCs in hexane with different sizes are obtained to be about 1.8 ms, which are the longest one in the reported Mn2+ in CsPbCl3 NCs.4-11,15,18 The Mn2+ doped CsPbCl3 NCs had a single exponential decay with a lifetime of up to 1.8 ms at the doping concentration of about 3% and a 8

ACS Paragon Plus Environment

Page 9 of 26 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

The Journal of Physical Chemistry

multi-exponential decay with a reduced lifetime with increasing the doping concentration, originating from radiative recombination of isolated Mn2+ ions and Mn2+-Mn2+ dimers.15 Therefore, the emission bands at 598 nm in all Mn2+ doped CsPbCl3 NC samples can be attributed to isolated Mn2+ ions. The PL QYs of Mn2+ in the doped NCs with different sizes are plotted in Figure 1e. The maximum PL QY is over 50% for the Mn2+ doped NCs with exciton emission of 400 nm while it is only 20% for the doped NCs with exciton emission of 397 nm, which may be related to amount of defects/traps in the doped NCs with small size. The corresponding PL QYs of exciton emissions in doped NCs with varied sizes were also summarized in Table S1. The experimental result indicates that the PL lifetimes of Mn2+ in the doped CsPbCl3 NCs are nearly the same despite a significant difference among PL QYs of the doped NCs with varied sizes.

Figure 2. TEM images and XRD patterns of Mn2+:CsPbCl3 NCs for NC397, 400, 403, 406, and 409. The inset in (c) shows a HRTEM image. 9

ACS Paragon Plus Environment

The Journal of Physical Chemistry 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 10 of 26

The TEM images and XRD patterns of Mn2+:CsPbCl3 NCs are shown in Fig. 2. As seen in Figure 2a, b, c, d, and e, the Mn2+:CsPbCl3 NCs exhibit a significant increase in size for NC397, 400, 403, 406, and 409 with increasing the reaction temperature from 130 °C to 210 °C and a relatively narrow size distribution. These monodispersed doped NCs have cubic morphology. The lattice spacing in the high resolution TEM (HRTEM) image of a NC for NC403 is clearly seen in the inset of Figure 2h, suggesting the NCs with a good crystallinity. The corresponding histograms of the Mn2+:CsPbCl3 NCs are shown in Fig. 2f, g, h, i, and j, respectively. The NC size distribution spectra are fitted with a Gaussian line shape. The average sizes of Mn2+:CsPbCl3 NCs for NC397, 400, 403, 406, and 409 are determined to be 5.31±0.55, 7.23±0.45, 8.74±0.60, 13.35±1.16, and 17.42±1.58 nm, respectively. Further the Mn2+:CsPbCl3 NCs with different sizes have a cubic structure (#75-0411) as seen in Figure 2k. It can be found that there are two relatively obvious diffraction peaks at 15.8 and 31.9 degree, which correspond to (100) and (200) directions, respectively, which are well consistent with our previous report.15 The diffraction peaks Mn2+:CsPbCl3 NCs with different sizes do not show a clear shift after introduction of Mn2+ dopants despite the remarkable broadening of diffraction peaks with the reduction of NC size.4

10

ACS Paragon Plus Environment

Page 11 of 26 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

The Journal of Physical Chemistry

Figure 3. Variable-temperature PL spectra (a), intensities (b), decay curves (c) and lifetimes (d) of Mn2+ in NC403 film or Mn2+ doped NC with different NC size. The excitation wavelength is 330 nm.

In order to study the size effects of Mn2+ luminescence properties in the Mn2+:CsPbCl3 NCs, the variable-temperature luminescence spectra and decay curves of Mn2+ and band edge emissions in Mn2+:CsPbCl3 NC samples were measured. Figure 3 shows the representative variable-temperature PL spectra and decay curves of Mn2+ in CsPbCl3 NC films deposited on silicon substrates for NC403 and the integrated PL intensities and lifetimes for all the doped NCs. The variable-temperature PL spectra and decay curves of band edge emissions in Mn2+:CsPbCl3 NC films and the integrated PL intensities, peak energies, FWHMs for all Mn2+:CsPbCl3 NCs are shown in Figures S1 and S2 in Supporting Information. As seen in Figure 3a and b, the Mn2+ PL is quite weak at 80 K. The PL intensity for NC397 gradually increases with increasing temperature to 260 K and then decreases rapidly. The maximum luminescence intensity at 260 K is about 13 times the initial intensity at 80 K. The enhancement of Mn2+ emission from 4T1 to 6A1 has been explained by the thermally activated exciton fission and energy transfer from host to Mn2+ ions.15 The PL 11

ACS Paragon Plus Environment

The Journal of Physical Chemistry 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 12 of 26

quenching of Mn2+ at high temperature is probably related to thermal degradation of the doped NCs due to defect/trap formation. Similar enhanced PL intensities with increasing temperature are observed for the other samples, in good agreement with our previous report.15 However, the maximum PL intensities of Mn2+ are observed at 260, 260, 280, 300, and 340 K for NC397, 400, 403, 406, and 409, respectively, as shown in Figure 3b. The size dependence of Mn2+ PL intensities below 300 K is not clearly understood, which is perhaps related to size-dependent localized charges within the band gap of doped NCs or exciton fission, resulting in long lifetime band edge emissions as seen in Figure S2. The peak energies of Mn2+ doped in these CsPbCl3 NCs are located at 2.05-2.08 eV at 300 K as seen in Figure S3 in Supporting Information. The emission band of Mn2+ ions for NC403 shifts to the blue about 78 meV with increasing temperature from 80 K to 360 K. The observed blue shift of the Mn2+ PL with increasing temperature is attributed to the decrease in crystal-field strength caused by thermal expansion of the host lattice, which is similar to Mn2+:ZnS and Mn2+:ZnSe NCs.21-25 As seen in Figure S3, the FWHM of Mn2+ in CsPbCl3 NCs is clearly broadened for small sized NCs perhaps due to the interaction among NCs during the film fabrication. The FWHMs for all NCs in solutions are quite similar as seen in Figure 1. The study for the widening mechanism of FWHMs is needed further. The FWHM of Mn2+ emission for NC403 gradually broadens from 181 meV to 305 meV with the increase of temperature from 80 K to 360 K. The FWHM broadening of Mn2+ is considered to originate from the electron-phonon coupling in the doped NCs.29,30 12

ACS Paragon Plus Environment

Page 13 of 26 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

The Journal of Physical Chemistry

As seen in Figure 3c and d, the PL decays of Mn2+ ions are gradually shortened with the increase of temperature, in contrast to their enhanced PL intensities. The PL decay curves of Mn2+ ions in CsPbCl3 NCs with varied sizes were fitted to estimate the average fluorescence lifetimes at low and high temperatures with a single- or three-exponential function, respectively. The PL lifetime of Mn2+ for NC403 decreases from 3.57 ms at 80 K to 1.66 ms at room temperature 300 K. It is surprisingly noted that the PL lifetimes of Mn2+ for the other NCs almost have similar temperature dependence from 80 K to 320 K. It is well known that the emissions of Mn2+ are considered to originate from the Mn2+ 4T1→6A1 d−d transition through energy transfer of excitons in hosts to dopants. Due to the spin-forbidden Mn d−d transition, the lifetime of Mn2+ emission is very long, which is in the range of microand milli-seconds.38-43 Meanwhile the ultrafast energy transfer occurring within picosecond-nanosecond range will have no effect on the Mn2+ PL decay dynamcs.13,46,47 So the Mn2+ PL lifetime in general can be decided by the coordination environment and the strength of the ligand field around Mn2+ such as Mn2+ doping concentration and the size of doped NCs. The experimental result may mean that the all Mn2+ ions in CsPbCl3 NCs with different size have uniform environment because the crystallization in ionic perovskite NCs is excellent under low concentration doping condition. On the other hand, the small red shift of band edge emissions for the doped NCs is 93 meV when the NC size is varied from 5.3 nm to 17.4 nm because the sizes of CsPbCl3 NCs are larger than the exciton Bohr radius of 2.5 nm, indicating a weak quantum confinement effect.44 In addition, no significant change in lattice 13

ACS Paragon Plus Environment

The Journal of Physical Chemistry 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 14 of 26

constant of CsPbCl3 NCs is demonstrated in the XRD experiment. Therefore the weak size dependence of Mn2+ PL energies and lifetimes indicates that the Mn2+ ions with nearly the same crystal field environment are homogeneously distributed in CsPbCl3 NCs.

Figure 4. PL spectra and decay curves of Mn2+ in CsPbCl3 NC films deposited on silicon substrates for NC400 (a, b) and NC409 (c, d) without/with heat treatment at 320, 340, 360, 380, and 400 K for 20 min. The PL spectra and decay curves of the samples were measured at room temperature after they cooled down. The PL intensities of band edge emissions are normalized.

The thermal degradation of Mn2+ emissions in CsPbCl3 NCs above 320 K can be better understood by monitoring the change in their unique PL spectra and lifetimes at room temperature. The PL spectra and decay curves of Mn2+:CsPbCl3 doped NC films for NC400 and NC409 without/with heat treatment at 320, 340, 360, 380, and 400 K for 20 min are shown in Figure 4. The normalized PL spectra of exciton and Mn2+ emissions in Mn2+:CsPbCl3 NC films for NC400 and 409 under heat treatment at various temperatures are shown in Figure S4 in Supporting Information. As seen in Figure 4a and c as well as Figure S4, it is clearly observed that the band edge emissions for NC400 and NC409 shifts to longer wavelength under higher heat treatment temperature over 360 K, indicating the size growth of doped NCs.47,48 The 14

ACS Paragon Plus Environment

Page 15 of 26 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

The Journal of Physical Chemistry

Mn2+ PL bands not only shift to longer wavelength, but also have significantly shortened decays after the doped NC films were annealed at above 360 K, as seen in Figure 4b and d. The average PL lifetimes of Mn2+ in doped CsPbCl3 NCs for NC400 and 409 under heat treatment at various temperatures are shown in Figure S5 in Supporting Information. It is clearly observed that the PL lifetimes of Mn2+ for NC400 and 409 keep unchanged at temperature below 340 K while they are significantly reduced to 0.55 and 1.04 ms, respectively, from their initial value of 1.45 ms, at temperature ranging from 340 K to 400 K. The PL decay curves of Mn2+ were fitted by single- or three-exponential function to calculate the PL lifetimes of NC400 and 409 under low and high (over 340 K) heat treatment temperatures, respectively. Because a large number of defects were produced around Mn2+ ions with increase of heat treatment temperature, which reduced the PL lifetimes of Mn2+ and introduced multi-exponential PL decay of Mn2+ ions.9-11 This also indicates that largely sized Mn2+ doped CsPbCl3 NCs have better thermal stability than the small ones. In addition, the narrowed linewidths of diffraction peaks in XRD patterns of Mn2+:CsPbCl3 NC films for NC400 and 409 under heat treatment at various temperatures indicate the growth of NC size above 360 K as shown in Figure S6 in Supporting Information.

15

ACS Paragon Plus Environment

The Journal of Physical Chemistry 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 16 of 26

Figure 5. PL spectra (a, c), decay curves (b, d), intensities (e) and lifetimes (f) of Mn2+ in CsPbCl3 NC films deposited on silicon substrates for NC400 under heat treatment at 340 K and 360 K for various times.

The PL spectra and decay curves of Mn2+ in doped CsPbCl3 NC films for NC400 under heat treatment at 340 and 360 K for various times are shown in Figure 5. It is observed that the Mn2+ PL intensity for NC400 under heat treatment at 340 K rapidly decreases with increasing annealing time while its PL decay time of 1.54 ms almost keeps unchanged as seen in Figure 5a and b. However, under heat treatment at 360 K both PL intensity and decay time are significantly reduced with increasing annealing time as seen in Figure 5c and d. The PL lifetime for NC400 is reduced to 0.85 ms after heat treatment for 1 h from the initial value of 1.54 ms. The similar changes in PL intensities and decay times for NC409 are observed as shown in Figure S7 in Supporting Information. The TEM images of Mn2+:CsPbCl3 NCs for NC400 and 409 under heat treatment at 360 K for 20 min indicate the growth of NC size as shown in Figure S8 in Supporting Information, which is consistent with that of annealed 16

ACS Paragon Plus Environment

Page 17 of 26 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

The Journal of Physical Chemistry

CsPbBr3 NCs.48 The principal degradation mechanisms of CH3NH3PbI3 film were related to a defect-generation process that is highly localized on surfaces and interfaces.49,50 The thermal degradation of Mn2+ PL in doped CsPbCl3 NCs are discussed as follows. At the first stage the reduction in Mn2+ PL intensity is related to generation of surface defects as nonradiative recombination centers in doped NCs at low temperature range from room temperature to about 340 K. Simultaneously the PL lifetimes of Mn2+ almost keep a constant, indicating the environment of crystal field around Mn2+ is still not varied because the size of doped NCs is unchanged. At the second stage, the reduction in PL intensity is considered to result from formation of amount of surface defects as nonradiative recombination centers formed in the doped NCs due to the NC growth at temperature above 360 K. On the other hand, more Mn2+ ions that do not emit on the NC surface are doped into the grown NCs and then Mn2+-Mn2+ dimers are formed, resulting in red shifted Mn2+ emissions and shortened Mn2+ PL lifetimes.15,18 Therefore, the experimental results indicates that the Mn-Cl bond is thermally stable below 340 K for largely sized Mn2+ doped NCs.

4. CONCLUSIONS In summary, the PL properties of Mn2+ doped in CsPbCl3 NCs with different size have been studied by variable-temperature steady-state and time resolved PL spectroscopy. The Mn2+ doped NCs with low Mn2+ doping concentration were synthesized using reaction temperature to vary NC size from 5.3 nm to 17.4 nm. It was found that the Mn2+ emissions in all the doped NCs in hexane almost exhibited size-independent PL 17

ACS Paragon Plus Environment

The Journal of Physical Chemistry 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 18 of 26

wavelengths and single-exponentially decayed lifetimes of 1.8 ms at room temperature. Further the Mn2+ emissions in doped NC films almost had the same temperature dependence of PL lifetimes from 80 to 300 K while they had size-dependent PL lifetimes at temperature above 340 K due to thermal degradation. Based on the change in Mn2+ PL spectra and lifetimes, the degradation mechanisms of Mn2+ emissions were explained by the formation of amount of nonradiative recombination centers such as defects or traps in size-unchanged and grown NCs under higher temperature heat treatment. This study provides detailed understanding of the thermal stability of perovskite NCs for their applications in solid state lighting and displays. The improvement of thermal stability can be expected by passivating the NC surface to effectively suppress surface defects.

■ ASSOCIATED CONTENT Supporting Information The Supporting Information is available free of charge on the ACS Publications website at DOI: 10.1021/acs.jpcc. Temperature dependent PL spectra and decay curves of Mn2+ in CsPbCl3 NC films under heat treatment at various temperatures. XRD and TEM of Mn2+ doped CsPbCl3 NCs after heat treatment.

■ AUTHOR INFORMATION Corresponding Authors *E-mail: [email protected] 18

ACS Paragon Plus Environment

Page 19 of 26 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

The Journal of Physical Chemistry

*E-mail: [email protected]

ORCID Xi Yuan: 0000-0001-8731-216X Jialong Zhao: 0000-0001-9020-1436

Notes The authors declare no competing financial interest.

■ ACKNOWLEDGMENTS This work was supported by the National Natural Science Foundation of China (Nos. 11704152, 11774134, 21461006, and 51472053), National Key Research and Development Program of China (2016YFB0401701), and Development of Science and Technology of Jilin Province (20170520114JH).

■ REFERENCES 1. Kovalenko M. V.; Protesescu L.; Bodnarchuk M. I. Properties and potential optoelectronic applications of lead halide perovskite nanocrystals. Science 2017, 358, 745-750. 2. Akkerman Q. A.; Rainò G.; Kovalenko M. V.; Manna L. Genesis, challenges and opportunities for colloidal lead halide perovskite nanocrystals. Nature Mater. 2018, 17, 394–405. 3. Yang D. D.; Li X. M.; Zeng H. B. Surface chemistry of all inorganic halide perovskite nanocrystals: Passivation mechanism and stability. Adv. Mater. Interfaces 19

ACS Paragon Plus Environment

The Journal of Physical Chemistry 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 20 of 26

2018, 5, 1701662. 4. Liu W. Y.; Lin Q. L.; Li H. B.; Wu K. F.; Robel I.; Pietryga J. M.; Klimov V. I. Mn2+-doped lead halide perovskite nanocrystals with dual-color emission controlled by halide content. J. Am. Chem. Soc. 2016, 138, 14954–14961. 5. Parobek D.; Roman B. J.; Dong Y. T.; Jin H.; Lee E.; Sheldon M.; Son D. H. Exciton-to-dopant energy transfer in Mn-doped cesium lead halide perovskite nanocrystals. Nano Lett. 2016, 16, 7376–7380. 6. Liu H. W.; Wu Z. N.; Shao J. R.; Yao D.; Gao H.; Liu Y.; Yu W. L.; Zhang H.; Yang B. CsPbxMn1–xCl3 perovskite quantum dots with high Mn substitution ratio. ACS

Nano 2017, 11, 2239–2247. 7. Mir W. J.; Jagadeeswararao M.; Das S.; Nag A. Colloidal Mn-doped cesium lead halide perovskite nanoplatelets. ACS Energy Lett. 2017, 2, 537–543. 8. Lin C. C.; Xu K. Y.; Wang D.; Meijerink A. Luminescent manganese-doped CsPbCl3 perovskite quantum dots. Sci. Rep. 2017, 7, 45906. 9. Guria A. K.; Dutta S. K.; Adhikari S. D.; Pradhan N. Doping Mn2+ in lead halide perovskite nanocrystals: Successes and challenges. ACS Energy Lett. 2017, 2, 1014– 1021. 10. Swarnkar A.; Ravi V. K.; Nag A. Beyond colloidal cesium lead halide perovskite nanocrystals: Analogous metal halides and doping. ACS Energy Lett. 2017, 2, 1089– 1098. 11. Adhikari S. D.; Dutta S. K.; Dutta A.; Guria A. K.; Pradhan Dr. N.

Chemically

tailoring the dopant emission in manganese-doped CsPbCl3 perovskite nanocrystals. 20

ACS Paragon Plus Environment

Page 21 of 26 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

The Journal of Physical Chemistry

Angew. Chem. Int. Ed. 2017, 56, 8746–8750. 12. Huang G. G.; Wang C. L.; Xu S. H.; Zong S. F.; Lu J.; Wang Z. Y.; Lu C. G.; Cui Y. P. Postsynthetic doping of MnCl2 molecules into preformed CsPbBr3 perovskite nanocrystals via a halide exchange-driven cation exchange. Adv. Mater. 2017, 29, 1700095. 13. Rossi D.; Parobek D.; Dong Y. T.; Son D. H. Dynamics of exciton–Mn energy transfer in Mn-doped CsPbCl3 perovskite nanocrystals. J. Phys. Chem. C 2017, 121, 17143–17149. 14. Zou S. H.; Liu Y. S.; Li J. H.; Liu C. P.; Feng R.; Jiang F. L.; Li Y. X.; Song J. Z.; Zeng H. B.; Hong M. C.; Chen X. Y. Stabilizing cesium lead halide perovskite lattice through Mn(II) substitution for air-stable light-emitting diodes. J. Am. Chem. Soc.

2017, 139, 11443–11450. 15. Yuan X.; Ji S. H.; De Siena M. C.; Fei L. L.; Zhao Z.; Wang Y. J.; Li H. B.; Zhao J. L.; Gamelin D. R. Photoluminescence temperature dependence, dynamics, and quantum efficiencies in Mn2+-doped CsPbCl3 perovskite nanocrystals with varied dopant concentration. Chem. Mater. 2017, 29, 8003−8011. 16. Zhu J. R.; Yang X. L.; Zhu Y. H.; Wang Y. W.; Cai J.; Shen J. H.; Sun L. Y.; Li C. Z. Room-temperature synthesis of Mn-doped cesium lead halide quantum dots with high Mn substitution ratio. J. Phys. Chem. Lett. 2017, 8, 4167–4171. 17. Arunkumar P.; Gil K. H.; Won S.; Unithrattil S.; Kim Y. H.; Kim H. J.; Im W. B. Colloidal organolead halide perovskite with a high Mn solubility limit: A step toward Pb-free luminescent quantum dots. J. Phys. Chem. Lett. 2017, 8, 4161–4166. 21

ACS Paragon Plus Environment

The Journal of Physical Chemistry 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 22 of 26

18. De A.; Mondala N.; Samanta A. Luminescence tuning and exciton dynamics of Mn-doped CsPbCl3 nanocrystals. Nanoscale 2017, 9, 16722–16727. 19. Chen D. Q.; Fang G. L.; Chen X. Silica-coated Mn-doped CsPb(Cl/Br)3 inorganic perovskite quantum dots: Exciton-to-Mn energy transfer and blue-excitable solid-state lighting. ACS Appl. Mater. Interfaces 2017, 9, 40477–40487. 20. Parobek D.; Dong Y.; Qiao T.; Son D. H. Direct hot-injection synthesis of Mn-doped CsPbBr3 nanocrystals. Chem. Mater. 2018, 30, 2939–2944. 21. Bhargava R. N.; Gallagher D.; Hong X.; Nurmikko A. Optical properties of manganese-doped nanocrystals of ZnS. Phys. Rev. Lett. 1994, 72, 416–419. 22. Norris D. J.; Efros A. L; Erwin S. C. Doped nanocrystals. Science 2008, 319, 1776–1779. 23. Karan N. S.; Sarma D. D.; Kadam R. M.; Pradhan N. Doping transition metal (Mn or Cu) ions in semiconductor nanocrystals. J. Phys. Chem. Lett. 2010, 1, 2863–2866. 24. Pradhan N.; Sarma D. D. Advances in Light-emitting doped semiconductor nanocrystals. J. Phys. Chem. Lett. 2011, 2, 2818–2826. 25. Pradhan N.; Adhikari S. D.; Nag A.; Sarma D. D. Luminescence, plasmonic, and magnetic properties of doped semiconductor nanocrystals. Angew. Chem. Int. Ed.

2017, 56, 7038–7054. 26. Norris D. J.; Yao N.; Charnock F. T.; Kennedy T. A. High-quality manganese-doped ZnSe nanocrystals. Nano Lett. 2001, 1, 3–7. 27. Yang H.; Holloway P. H. Efficient and photostable ZnS-passivated CdS:Mn luminescent nanocrystals. Adv. Fucnt. Mater. 2004, 14, 152–156. 22

ACS Paragon Plus Environment

Page 23 of 26 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

The Journal of Physical Chemistry

28. Beaulac R.; Archer P. I.; Ochsenbein S. T.; Gamelin D. R. Mn2+-doped CdSe quantum dots: New inorganic materials for spin-electronics and spin-photonics. Adv.

Funct. Mater. 2008, 18, 3873–3891. 29. Zheng J. J.; Yuan X.; Ikezawa M.; Jing P. T.; Liu X. Y.; Zheng Z. H.; Kong X. G.; Zhao J. L.; Masumoto Y. Efficient photoluminescence of Mn2+ ions in MnS/ZnS core/shell quantum dots. J. Phys. Chem. C 2009, 113, 16969–16974. 30. Yuan X.; Zheng J. J.; Zeng R. S.; Jing P. T.; Ji W. Y.; Zhao J. L.; Yang W. Y.; Li H. B. Thermal stability of Mn2+ ion luminescence in Mn-doped core/shell quantum dots.

Nanoscale 2014, 6, 300–307. 31. Yang, Y. G.; Chen, O.; Angerhofer, A.; Cao, Y. C. J. Am. Chem. Soc. 2006, 128, 12428–12429. 32. Pradhan N.; Peng X. Efficient and color-tunable Mn-doped ZnSe nanocrystal emitters:  Control of optical performance via greener synthetic chemistry. J. Am.

Chem. Soc. 2007, 129, 3339–3347. 33. Pradhan N.; Goorskey D.; Thessing J.; Peng X. G. An alternative of CdSe nanocrystal emitters: Pure and tunable impurity emissions in ZnSe nanocrystals. J.

Am. Chem. Soc. 2005, 127, 17586–17587. 34. Hazarika A.; Layek A.; De S.; Nag A.; Debnath S.; Mahadevan P.; Chowdhury A.; Sarma D. D. Ultranarrow and widely tunable Mn2+-induced photoluminescence from single Mn-doped nanocrystals of ZnS-CdS alloys. Phys. Rev. Lett. 2013, 110, 267401. 35. Nag A.; Cherian R.; Mahadevan P.; Gopal A. V.; Hazarika A.; Mohan A.; Vengurlekar A. S.; Sarma D. D. Size-dependent tuning of Mn2+ d emission in 23

ACS Paragon Plus Environment

The Journal of Physical Chemistry 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 24 of 26

Mn2+-doped CdS nanocrystals: Bulk vs surface. J. Phys. Chem. C 2010, 114, 18323– 18329. 36. Ithurria S.; Guyot-Sionnest P.; Mahler B.; Dubertret B. Mn2+ as a radial pressure gauge in colloidal core/shell nanocrystals. Phys. Rev. Lett. 2007, 99, 265501. 37. Hazarika A.; Pandey A.; Sarma D. D. Rainbow emission from an atomic transition in doped quantum dots. J. Phys. Chem. Lett. 2014, 5, 2208–2213. 38. Bol A. A.; Meijerink A. Long-lived Mn2+ emission in nanocrystalline ZnS:Mn2+.

Phys. Rev. B 1998, 58, R15997–16000. 39. Suyver J. F.; Wuister S. F.; Kelly J. J.; Meijerink A. Luminescence of nanocrystalline ZnSe:Mn2+. Phys. Chem. Chem. Phys. 2000, 2, 5445–5448. 40. Ishizumi A.; Kanemitsu Y. Luminescence spectra and dynamics of Mn-doped CdS core/shell nanocrystals, Adv. Mater. 2006, 18, 1803–1085. 41. Gan C. L.; Zhang Y. P.; Battaglia D.; Peng X. G.; Xiao M. Fluorescence lifetime of Mn-doped ZnSe quantum dots with size dependence. Appl. Phys. Lett. 2008, 92, 241111. 42. Yang B. P.; Shen X. C.; Zhang H. C.; Cui Y. P.; Zhang J. Y. Luminescent and magnetic properties in semiconductor nanocrystals with radial-position-controlled Mn2+ doping. J. Phys. Chem. C 2013, 117, 15829–15834. 43. Pu C. D.; Ma J. L.; Qin H. Y.; Yan M.; Fu T.; Niu Y.; Yang X. L.; Huang Y. F.; Zhao F.; Peng X. G. Photoluminescence decay dynamics in microsecond to millisecond range: Synthesis and applications. ACS Cent. Sci. 2016, 2, 32–39. 44. Protesescu L.; Yakunin S.; Bodnarchuk M. I.; Krieg F.; Caputo R.; Hendon C. H.; 24

ACS Paragon Plus Environment

Page 25 of 26 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

The Journal of Physical Chemistry

Yang R. X.; Walsh A.; Kovalenko M. V. Nanocrystals of cesium lead halide perovskites (CsPbX3, X = Cl, Br, and I): Novel optoelectronic materials showing bright emission with wide color gamut. Nano Lett. 2015, 15, 3692–3696. 45. Cao, S.; Li, C.; Wang, L.; Shang, M.; Wei, G.; Zheng, J.; Yang, W. Long-lived and well-resolved Mn

2+

ion emissions in CuInS-ZnS quantum dots. Sci. Rep. 2015, 4,

7510. 46. Fang H. H.; Wang F.; Adjokatse S.; Zhao N.; Even J.; Loi M. A. Photoexcitation dynamics in solution-processed formamidinium lead iodide perovskite thin films for solar cell applications. Light: Sci. Appl. 2016, 5, e16056. 47. Chen H. Y.; Maiti S.; Son D. H. Doping location-dependent energy transfer dynamics in Mn-doped CdS/ZnS nanocrystals. ACS Nano 2012, 6, 583–591. 48. Yuan X.; Hou X. M.; Li J.; Qu C. Q.; Zhang W. J.; Zhao J. L.; Li H. B. Thermal degradation of luminescence in inorganic perovskite CsPbBr3 nanocrystals. Phys.

Chem. Chem. Phys. 2017, 19, 8934–8940. 49. Deretzis I.; Smecca E.; Mannino G.; Magna A. L.; Miyasaka T.; Alberti A. Stability and degradation in hybrid perovskites: Is the glass half-empty or half-full. J.

Phys. Chem. Lett. 2018, 9, 3000–3007. 50. Weerd C. De.; Gregorkiewicz T.; Gomez L. All-inorganic perovskite nanocrystals: microscopy insights in structure and optical properties. Adv. Opt. Mater. 2018, 6, 1800289.

25

ACS Paragon Plus Environment

The Journal of Physical Chemistry 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 26 of 26

TOC GRAPHIC

26

ACS Paragon Plus Environment