Preparation and characterization of proteinloaded electrospun fiber mat and its release kinetics Peng Wen, Yan Wen, Xiao Huang, Minhua Zong, and Hong Wu J. Agric. Food Chem., Just Accepted Manuscript • Publication Date (Web): 23 May 2017 Downloaded from http://pubs.acs.org on May 24, 2017
Just Accepted “Just Accepted” manuscripts have been peer-reviewed and accepted for publication. They are posted online prior to technical editing, formatting for publication and author proofing. The American Chemical Society provides “Just Accepted” as a free service to the research community to expedite the dissemination of scientific material as soon as possible after acceptance. “Just Accepted” manuscripts appear in full in PDF format accompanied by an HTML abstract. “Just Accepted” manuscripts have been fully peer reviewed, but should not be considered the official version of record. They are accessible to all readers and citable by the Digital Object Identifier (DOI®). “Just Accepted” is an optional service offered to authors. Therefore, the “Just Accepted” Web site may not include all articles that will be published in the journal. After a manuscript is technically edited and formatted, it will be removed from the “Just Accepted” Web site and published as an ASAP article. Note that technical editing may introduce minor changes to the manuscript text and/or graphics which could affect content, and all legal disclaimers and ethical guidelines that apply to the journal pertain. ACS cannot be held responsible for errors or consequences arising from the use of information contained in these “Just Accepted” manuscripts.
Journal of Agricultural and Food Chemistry is published by the American Chemical Society. 1155 Sixteenth Street N.W., Washington, DC 20036 Published by American Chemical Society. Copyright © American Chemical Society. However, no copyright claim is made to original U.S. Government works, or works produced by employees of any Commonwealth realm Crown government in the course of their duties.
Page 1 of 46
Journal of Agricultural and Food Chemistry
1
Preparation and characterization of protein-loaded electrospun fiber
2
mat and its release kinetics
3
Peng Wen1#, Yan Wen1#, Xiao Huang1, Min-Hua Zong1, Hong Wu1,2* 1
4
School of Food Science and Engineering, South China University of Technology, Guangzhou 510640, China
5 2
6
Guangdong Province Key Laboratory for Green Processing of Natural Products and Product Safety, Guangzhou 510640, China
7 8 9 10 11 12 13 14 15 16 17 18
*To whom correspondence should be addressed. Tel.: +86-20-22236669;
19
E-mail:
[email protected] (H. Wu)
20
#
This authors have the same contribution and are co-first author
21 22 1
ACS Paragon Plus Environment
Journal of Agricultural and Food Chemistry
23
ABSTRACT
24
For the enhancement of protein’s bioavailability, a specific delivery system was
25
developed by coaxial electrospinning. Bovine serum albumin (BSA) was used as
26
protein model and the core-sheath fiber mat was fabricated using sodium alginate as
27
shell layer and the BSA-loaded chitosan nanoparticle that prepared previously as core
28
layer. By optimizing electrospinning parameters, uniform fibers with diameters ranging
29
from 200 nm to 600 nm were obtained, and transmission electron microscopy and
30
confocal laser scanning microscopy revealed its core-sheath structure. Fourier
31
transform infrared spectroscopy (FTIR) analysis demonstrated that there existed
32
molecular interaction between components, which enhanced the mat’s thermal stability
33
and mechanic property. It was found that the predominant release mechanism of BSA
34
from fiber mat was erosion, and little change was occurred in the secondary structure
35
of encapsulated BSA indicated by FTIR and circular dichroism analysis. The study
36
shows that the obtained fiber mat is a potential delivery system for protein.
37 38 39 40 41 42
KEYWORDS: coaxial electrospinning, core-sheath fiber, protein, release kinetics,
43
stability
44 2
ACS Paragon Plus Environment
Page 2 of 46
Page 3 of 46
Journal of Agricultural and Food Chemistry
45
INTRODUCTION
46
Recently, with the increased demands for improving human health through
47
diet, bioactive proteins have gained tremendous attention for their health
48
benefits.1,2 However, their oral bioavailability are still very low due to the
49
significant barriers in the upper gastrointestinal tract (GIT), including
50
acid-catalyzed degradation in the stomach, proteolytic degradation by digestive
51
enzymes in the small intestine, and poor intestinal membrane permeability etc.3
52
Hence, an effective delivery approach that can enhance bioavailability and
53
preserve biological activity of protein is desirable.
54
Increased progress have been made over the years to improve the
55
bioavailability of protein, including the use of protease inhibitors or absorption
56
enhancers, muco-adhesive polymeric delivery systems, chemical modification of
57
macromolecules, nano/micro-particulate systems and the site-specific delivery to
58
the colon etc.4 Among them, the colon-specific delivery of protein is more
59
attractive since colon offers a near neutral pH, prolonged transit time, reduced
60
digestive enzymatic activity, abundant microflora (1011-1012 CFU/mL), and
61
higher receptiveness of protein through colonic epithelia,5 which is desired not
62
only for improving the oral bioavailability of protein, but also for treating colon
63
diseases. Especially, the inability of upper GIT enzymes to digest certain
64
polysaccharides (such as pectin, dextran, chitosan etc) is taken advantage of
65
developing a colon-specific delivery system. The protein can be encapsulated
66
into these polysaccharides, as expected, the hydrolytic enzymes that secreted by 3
ACS Paragon Plus Environment
Journal of Agricultural and Food Chemistry
Page 4 of 46
67
microflora are responsible for degradation of carriers, which leads to the release
68
of protein in the colon.6 Hence, efforts have been made to prepare
69
polysaccharide-based colonic delivery system for protein.6-8
70
Regarding the methods for constructing delivery system, electrospinning, a
71
simple and cost-effective technique, has been recognized as a promising
72
approach
73
demonstrated that electrospun fibers can improve the encapsulation efficiency,
74
bioactivity and oral bioavailability of bioactive compounds.12,13 Moreover, a
75
number of publications have revealed the developments in modified
76
electrospinning, such as the tri-axial electrospinning,14 the modified coaxial
77
electrospinning,15 and the side-by-side electrospinning 16 techniques et al., which
78
expand the capability of electrospinning in generating nano-products and could
79
further
80
electrospinning process by confining it into the core.17 Owing to these merits,
81
electrospinning has been well established for small molecule drug delivery in the
82
pharmaceutical fields,18 however, its application in food industry is less
83
investigated.19-21
to
encapsulate
protect
the
bioactive
fragile
compounds.9-11
bioactive
compounds
Previous
from
the
study
stress
has
of
84
Sodium alginate (SA) can resist gastric acid, and chitosan (CS) is insoluble in
85
small intestine and can be degraded by microbial enzymes in colon, thus, the
86
combination of both can potentially be used to prepare colon-specific delivery
87
system. Hence, in this study, bovine serum albumin (BSA) was chosen as the
88
protein model and it was encapsulated into CS nanoparticle by ionic gelation. 4
ACS Paragon Plus Environment
Page 5 of 46
Journal of Agricultural and Food Chemistry
89
Then, the electrospun fiber mat loaded with BSA was fabricated by coaxial
90
electrospinning using SA as shell layer and the BSA-loaded CS nanoparticle as
91
core layer to increase the oral availability of protein. The preparation process
92
was systematically studied by investigating the influence of solution property
93
and processing parameters on the nanofiber morphology through scanning
94
electron microscopy (SEM). Moreover, the electrospun solution property, and
95
the morphologies, structures, functional performance of final core-sheath
96
product, as well as the bioactivity and release profile of BSA from the obtained
97
fiber mat were characterized in details.
98
MATERIALS AND METHODS
99
Materials. Sodium alginate (SA, from brown algae), β-glucosidase (≥6 U/mg) and
100
sodium tripolyphosphate (TPP) were purchased from Sigma-Aldrich company
101
(Shanghai, China); Chitosan (CS, 160 kDa, DD was 87%) was provided by Dacheng
102
Biotech. Co. Ltd. (Weifang, China); polyoxyethylene (PEO, 100 kDa), pepsin (1:3000)
103
and trypsin (1:250) were obtained from Aladdin biological technology Co., Ltd.
104
(Shanghai, China); polyvinyl alcohol (PVA, Mw: 85000-124000) was purchased from
105
Tianma fine chemical factory (Guangzhou, China). BSA was obtained from Shanghai
106
biological technology Co. Ltd. (Shanghai, China). Folin−ciocalteu reagent was
107
purchased from Qiyun biological technology Co., Ltd. (Guangzhou, China). Deionized
108
water was used to prepare all the solutions.
109
Preparation and characterization of electrospinning solution. A series
110
concentrations of shell solution was prepared by dissolving a certain amount of SA and 5
ACS Paragon Plus Environment
Journal of Agricultural and Food Chemistry
111
PEO in water/pure ethanol (90:10, v/v) under constant stirring for 24 h. The viscosity
112
and conductivity of the above solution was measured by Brookfield viscometer (Model
113
DV-II + Pro, Brookfield Engineering Laboratories Inc., Stouchton, USA) and a
114
conductivity meter (DDS-11A, Leici Instrument Co., Shanghai, China), respectively.
115
Surface tension was determined using a pendant drop analyzer from SEO Co. Ltd
116
(model Phoenix 300, Lathes, South Korea). Rheological experiment was performed
117
with a stress-controlled rheometer (AR2000, TA Instruments Inc., New Castle, USA).
118
For core solution, BSA-loaded CS nanoparticle was firstly prepared using ionic
119
gelation with some modifications.22 9 mL of CS solution (3 mg/mL, dissolved in 1%
120
acetic acid) that adjusted for pH 5.3 previously was mixed with 1 mL of BSA solution
121
(1.5 mg/mL, dissolved in 1% water). The nanoparticle was formed as the TPP solution
122
(1 mg/mL in water) was added into the above BSA-CS solution in a rate of 400 µL/min)
123
to achieve a mass ratio of 4:1 for CS:TPP. Then, a mixed solution composed of the
124
above BSA-loaded CS nanoparticle suspension and PVA (6% w/w, dissolved in water)
125
in different volume ratios comprised the core solution.
126
Electrospinning process. Electrospinning was conducted by applying a voltage
127
varying from 14 to 20 kV with a power supply (ES50P-5W/DAM, Gamma, USA).
128
Two syringe pumps (NE-300, New Era Pump Systems Inc., USA) and a homemade
129
concentric spinneret (a 17 gauge for shell and 21 gauge for core) were adopted to give
130
the shell fluid and core fluid flow rate ranging from 0.2 mL/h to 0.6 mL/h, respectively.
131
A grounded collecting plate was used for fiber deposition. The distance between needle
132
tip and collector was varied from 14 cm to 18 cm. During the electrospinning, the 6
ACS Paragon Plus Environment
Page 6 of 46
Page 7 of 46
Journal of Agricultural and Food Chemistry
133
temperature was 25±1oC and the relative humidity was around 35~40%. The obtained
134
fiber mat was dried in a desiccator before analysis.
135
Characterization of electrospun fiber mat. The morphology of nanofiber was
136
observed by SEM (Zeiss EVO 18, Carl Zeiss Jena, Germany), and the fiber diameter
137
distribution was calculated by analysis of around 50 fibers from the SEM image. The
138
surface morphology of the fiber mat was also characterized using AFM (Nanoscope
139
IIIa, Digital Instruments Inc., Santa Barbara, USA). The scanned area was 8 µm × 8
140
µm and the image was processed using the Nanoscope software. For the observation of
141
core-sheath structure of fibers by TEM (JEM-2010, JEOL Ltd., Tokyo, Japan), a very
142
thin layer of electrospun fibers on the grid was prepared by putting the copper grid
143
onto the collector, and then the fibers were directly deposited on the grid during the
144
electrospinning process.
145
To study the distribution of each component, SA and CS was labeled with
146
fluorescein isothiocynate (SA-FITC) and Rhodamine (CS-RhB), respectively. These
147
labeled polymers were mixed with neat polymers to prepare electrospun fiber mat and
148
the core-sheath structure was examined using CLSM (LSM 510 META, Carl Zeiss Inc.
149
USA). Briefly, CS-RhB was prepared by dissolving 100 mg of CS in 10 ml of
150
0.1mol/L acetic acid, and then 10 ml of methanol and 3.25 ml of 2 mg/mL RhB in
151
methanol were added into the above CS solution followed by reacting overnight.
152
SA-FITC was prepared by mixing 100 ml of 17.6 mg/mL SA with 10 mL of 1.77
153
mg/mL FITC in methanol at 4oC for 1 d. CS-RhB and SA-FITC were purified via
154
dialysis, freeze dried and stored at 4oC until use, respectively. 7
ACS Paragon Plus Environment
Journal of Agricultural and Food Chemistry
155
The interaction between the components was investigated using FTIR. All samples
156
were recorded on a Bruker Model Equinox 55 FTIR spectrophotometer (Bruker Co.,
157
Ettlingen, Germany). For electrospun fibers, ATR was used. While for the released
158
BSA, KBr disk was adopted. The FTIR was performed in the mean infrared region
159
with a wavenumber range of 4000-500 cm -1 and spectral resolution of 4 cm -1.
160
The thermal stability of different sample was evaluated by TGA. It was performed
161
from room temperature to 700oC, at a heating rate of 10oC/min and under nitrogen
162
atmosphere (Q500, TA Instruments Inc., New Castle, USA).
163
The physical form of components in the fiber was conducted using XRD (model D8
164
Advance, Bruker Co., Germany) with Cu Kα radiation (λ = 0.15406nm) accelerated at
165
voltage and current of 40 kV and 40 mA, respectively. The XRD pattern was collected
166
from 5° to 60° at an increment of 0.02° per 0.5 s.
167
The mechanical property of electrospun fiber mat was determined at 25 °C using a
168
universal testing machine (INSTRON 5565, Instron Co., Canton, USA) according to
169
ASTM standard method D882. Film was cut into strip (10 × 2.5 cm) and conditioned
170
in desiccator with saturated NaBr solution (58% relative humidity) for 48 h prior to the
171
test. The thickness of film was measured by a micrometer. The strip was mounted
172
between the corrugated tensile grip of the instrument and the initial grip spacing and
173
cross-head speed were set at 50 mm and 0.5 mm/s, respectively. A strain rate of 2
174
mm/min was used throughout the experiment. Three replications of each sample were
175
performed and average value of the measurement was used.
8
ACS Paragon Plus Environment
Page 8 of 46
Page 9 of 46
Journal of Agricultural and Food Chemistry
176
BSA release profile and the diffusion coefficient. The release studies of BSA from
177
fiber mat under simulated digestive fluids were performed using a dissolution rate test
178
apparatus (RCZ-8B, Tianda Tianfa Co., Ltd., Tianjing, China) (100 rpm, 37°C)
179
according to the USP23 method. Simulated gastric fluid containing 10 mg/mL pepsin
180
(SGF, pH 1.2) was prepared by 0.1 mol/L HCl; simulated intestinal fluid containing 10
181
mg/mL trypsin (SIF, pH 6.8) and simulated colonic fluid containing β-glucosidase
182
(SCF, pH 7.4) were prepared by phosphate buffer solution. At predetermined time
183
interval, 1 mL of medium was sampled and replaced by an equal volume of fresh
184
medium. The BSA content in the sample was calculated using different calibration
185
curve of BSA that previously determined and standardized in different dissolution
186
medium (Figure S1).
187 188
The release profiles were fitted according to Higuchi and Ritger–Peppas model (equation 1 and 2) to describe the release mechanism.
==kt1/2
189
Higuchi:
190
Ritger-peppas:
(1)
==ktn
(2)
191
(where Mt/M∞ is the accumulated fraction of BSA release in time t;
k is the
192
release rate constant; n is the release exponent indicating release mechanism).
193
Additionally, the diffusion coefficients of BSA from fiber mat under different
194
simulated digestive fluids were also calculated using the short-time and long-time
195
approximation equations (equation 3 and 4), respectively.23
196
short time:
197
long time:
= ;
= exp (−
(3)
);
(4) 9
ACS Paragon Plus Environment
Journal of Agricultural and Food Chemistry
198
(where D is the diffusion coefficient, L0 is the mat’s thickness).
199
The stability of BSA. Secondary structure characterization of BSA was performed
200
by FTIR and CD. Before the test, the lyophilized powder of BSA loaded CS
201
nanoparticle and the obtained electrospun fiber mat were immersed into incubation
202
mixture (0.1 mol/L phosphate buffer solution, pH6.8) for 48 h to obtain released BSA.
203
For FTIR measurement, the incubation supernatant containing BSA was dropped onto
204
the thin piece of KBr. The secondary structure of BSA was estimated quantitatively
205
from the amide I band (1700-1600 cm-1) by a curve-fitting program. The CD
206
measurement of BSA was recorded in the range 190–260 nm at a protein concentration
207
of 0.1 mg/mL, using a Chirascan spectropolarimeter (Applied Photophysics, UK). A
208
quartz cylindrical cell of 1 cm path length was used for the measurement. The native
209
BSA was used as control. To calculate the secondary structural contents of BSA, the
210
CD spectra were analyzed by a curve fitting programme of software CD Pro using
211
SELCON method, as described by Sreerama and Woody.24
212
Statistical analysis. Data was obtained at least in triplicate (n = 3), and was
213
expressed as mean±standard deviation (SD). Statistical analysis was performed
214
using one way analysis of variance (ANOVA). A value of P ≤ 0.05 was
215
considered statistically significant.
216
RESULTS AND DISCUSSION
217
Preparation of electrospun fiber mat. In order to achieve colon-specific delivery
218
of protein, core-sheath structured electrospun fiber mat was prepared by using SA as
219
the shell layer to resist gastric acid in SGF and BSA-loaded CS nanoparticle as core 10
ACS Paragon Plus Environment
Page 10 of 46
Page 11 of 46
Journal of Agricultural and Food Chemistry
220
layer that can be degraded by microbial enzymes in SCF. Unfortunately,
221
electrospinning of SA was unsuccessful due to its rigid structure, a surfactant and
222
second material was added to improve the electrospinnability of SA.25 In this study, the
223
impacts of surfactant and PEO on the solution properties and the morphology of
224
obtained nanofibers were investigated (Table 1 and Figure 1). As shown in Figure 1, it
225
was observed that the addition of surfactant led to the morphological transmission from
226
beaded fibers to uniform fibers under the same mass ratio of SA to PEO, especially for
227
2% Pluronic F127. This was because the addition of surfactant could increase the
228
viscosity, and reduce the conductivity and surface tension of SA solution, which was in
229
favor of forming fibers (Table 1). However, the use of toxic surfactant Trition X-100
230
limited its application, thus, Pluronic F127, an FDA-approved surfactant, was selected
231
as the appropriate surfactant. It was also observed that the more PEO content, the less
232
beaded fibers. In order to obtain uniform fibers and maximize the content of SA, the
233
mass ratio of SA to PEO was chosen as 80:20.
234
Besides surfactant and mass ratio of SA to PEO, the impact of shell polymer’s
235
concentration on fiber morphology was also investigated (Figure 2). It showed that, to
236
some extent, the increase of concentration (from 7% to 9%, w/w) was favorable for the
237
formation of uniform fibers, whereas higher concentration (10%, w/w) resulted in
238
larger fiber diameter distribution. The optimized concentration of shell polymer was 9%
239
(SA: PEO=80:20). That was because PEO can interact with SA by forming
240
inter-molecular hydrogen bonding, leading to the improved chain entanglement and
241
flexibility, while higher concentration (more chain entanglement) caused less 11
ACS Paragon Plus Environment
Journal of Agricultural and Food Chemistry
242
stretching of the jet thus producing larger nanofibers. Rheological measurement was
243
further applied to study the effect of polymer concentration on the chain
244
conformation.25 As shown in Figure 3a, storage modulus (G’) and loss modulus (G’’)
245
had a tendency to approach each other at higher concentration, suggesting that the
246
chain entanglement between SA and PEO was enhanced.26 Additionally, the apparent
247
flexibility of SA chain was increased as the shear-thinning behavior of shell solution
248
enhanced considerably at higher concentration in the shear rate of 0.1–100 s−1 (Figure
249
3b). Therefore, the rheological measurements suggested that the beaded fibers
250
produced by shell solution with concentration < 9% can be due to the insufficient chain
251
entanglement.27
252
As described above, the combination of SA as shell layer and CS as core layer were
253
used to achieve the colon-specific delivery of protein. However, similar with SA, the
254
electrospinning of CS is difficult due to its high conductivity, hence, PVA was added to
255
improve the electrospinnability of CS and the composition of core solution was
256
optimized to obtain uniform fibers. As depicted in Figure 4, beads were observed in the
257
electrospun CS/PVA fibers under volume ratios of 70:30 and 40:60, while uniform
258
nanofiber was obtained at ratios of 50:50 and 40:60. In order to obtain uniform fibers
259
and maximize CS content, the volume ratio of 50:50 for CS to PVA was adopted.
260
Apart from the solution composition, the impacts of electrospinning parameters on
261
the fiber morphology, including distance, voltage and flow rate, were also investigated
262
and the results were presented in Figure S2-4. From the SEM images and the
263
calculated diameter distribution, the optimal electrospinning conditions were voltage 12
ACS Paragon Plus Environment
Page 12 of 46
Page 13 of 46
Journal of Agricultural and Food Chemistry
264
17 kV, distance 16 cm and flow rate 0.3 mL/h, and the diameter distributions of
265
resulted core-sheath fiber mat were in the range of 200-600 nm.
266
Characterization of electrospun fiber mat. AFM was employed to characterize the
267
surface morphology of obtained electrospun fiber mat. As shown in Figure 5, the 2D
268
image revealed the fiber diameter ranging from 200 to 600 nm, which was consistent
269
with the previous SEM result. The 3D image exhibited the relatively smooth surface
270
with clear fibril structure.
271
The core-sheath structure of obtained fibers was then investigated by CLSM. As
272
shown in Figure 6, the shell fiber and core fiber exhibited green color and red color,
273
respectively, revealing the successful preparation of FITC-labeled SA and Rh
274
B-labeled CS. For the CLSM image of coaxial electrospun fibers, it emitted both green
275
and red fluorescence, which is an indication of the presence of FITC-labeled SA and
276
Rh B-labeled CS in the coaxial electrospun fibers. TEM was further conducted to
277
provide direct evidence that CS labeled with RhB was indeed encapsulated within the
278
shell material of SA labeled with FITC. As expected, a core-sheath structure fiber was
279
successfully constructed (Figure 6d), and the fibrous morphology without beads was
280
also consistent with SEM observation. It can be seen that both TEM and CLSM
281
revealed the core-sheath structure of obtained fibers.
282
FTIR was further carried out to investigate the peak shifts that could be attributed to
283
the interaction between components, such as hydrogen bonding (Figure 7). The
284
characteristic band of PEO at 1343 cm-1, 1122 cm-1 and 843 cm-1 was due to the -CH2
285
bond stretching, C–O–C asymmetric stretching and bending vibrations, respectively. 13
ACS Paragon Plus Environment
Journal of Agricultural and Food Chemistry
286
However, for SA/PEO electrospun mat, the band of hydroxyl stretching (3342 cm-1)
287
became much broader and the absorption band at 1122 cm-1 for original PEO shifted to
288
a lower wavenumber (1116 cm-1). This phenomenon indicated that the interaction
289
between SA and PEO was through hydrogen bonding, which was formed by hydroxyl
290
groups of SA and ether oxygen groups of PEO. Regarding the CS/PVA system, the
291
band at 3350 cm-1 (the OH stretching vibrations) of PVA had shifted toward lower
292
value (3338 cm-1) in CS/PVA electrospun fiber mat, suggesting the formation of
293
hydrogen bond between PVA and CS chains. In addition, the wavenumber of 1560
294
cm-1 observed in CS was owing to the N-H vibration, and it was shifted toward a lower
295
value (1543 cm-1) with the addition of PVA. This was another indication of hydrogen
296
bond between –OH of PVA and –NH of CS chains. Hence, the FTIR spectra of
297
SA/PEO and CS/PVA fiber mats demonstrated that there exist interactions between
298
different components.
299
XRD analyses were performed to monitor a possible change of crystallinity of
300
obtained electrospun fiber mat and assess the compatibility of different components.
301
As shown in Figure 8, the XRD patterns of SA showed broad peak, indicating its
302
amorphous nature, while the two sharp characteristic peaks of PEO powder at 18.9o
303
and 23.2o revealed its crystalline form. PVA had a strong peak at 19.6o with a small
304
shoulder at 22.4o and CS possessed two major peaks at 10.9o and 20.4o, respectively. It
305
was noted that after electrospinning, the PVA and PEO elctrospun fiber mats exhibited
306
a considerable reduction of crystallinity compared to the pure PEO and PVA powder,
307
respectively, indicating that crystalline structure can be influenced by electrospinning. 14
ACS Paragon Plus Environment
Page 14 of 46
Page 15 of 46
Journal of Agricultural and Food Chemistry
308
The depression of crystallization in electrospun fiber mat is commonly explained by
309
the
310
electrospinning that limited the development of crystallinity, similar result was also
311
observed by others.28 For SA/PEO electrospun fiber mat, besides the effect of
312
electrospinning process, the reduction of crystallinity was also resulted from the
313
diluting effect of amorphous SA. Additionally, for crystalline substances, the XRD
314
pattern is generally expressed as simply mixed patterns of different components if
315
there is no interaction between molecules or they have low compatibility as described
316
by other literatures.29,30 For the electrospun CS/PVA fiber mat, it exhibited a
317
considerable reduction of crystallinity as a decrease of peak intensity approximately at
318
10° and 20° was observed, which was probably caused by the reduction of
319
intramolecular hydrogen bonding of PVA and the formation of intermolecular
320
hydrogen bonding between PVA and CS.31,32 Nevertheless, the obtained core-sheath
321
fiber mat was still in crystalline nature. Since it had been reported that the folding of
322
polymer chains during crystallization can be interrupted by another polymer chains
323
when the two types of chains are miscible and interact closely,33 it can be inferred that
324
good compatibility was existed among different components.
polymer
dissolution
and
subsequently
rapid
solidification
process
of
325
Thermal Property. TGA was used to evaluate the thermal stability of polymeric
326
materials.34 The weight loss and its derivate curve were presented in Figure 9. As
327
decipted in Figure 9, SA/PEO electrospun fiber mat degraded in three steps and it was
328
evidenced by the distinct reaction peaks at around 63 oC, 240 oC and 408 oC in the
329
DTG curves.They were attributed to the evaporation of absorbed water, and the 15
ACS Paragon Plus Environment
Journal of Agricultural and Food Chemistry
330
thermal degradation of SA and PEO, respectively. Additionally, the thermal
331
degradation temperature of the fiber mat was slightly increased with increasing of PEO
332
content, as shown in Figure 9c and 9d. This may be correspond to the formation of
333
hydrogen bonding from the ether oxygen of PEO and the hydroxyl groups of SA.
334
Simialar results were reported by others.35 The thermal degradation of CS/PVA
335
electrospun mat was also presented in three stages, the second weight loss step at
336
200-350 oC was due to the thermal degradation of PVA and chitosan, and the third
337
weight loss step at 400-500 oC was owing to the degradation of the by-products
338
generated by PVA.36,37 In the range between 200 and 350 oC, CS showed more thermal
339
stability (lower weight loss) than PVA. Consequently, as the CS ratio increased in the
340
blend, the residual mass increased from 9% to 11% (Figure 9e). Similar results were
341
reported by Bonilla et al 38. Further, it was found that the addition of CS resulted in an
342
increase of decomposition temperature, indicating the interaction between PVA and CS
343
(Figure 9f). Similar results were observed by Lewandowska 36 and Peesan et al.39
344
Tensile property. Since film may be subjected to various kinds of stress being used,
345
the study of mechanical property is of primary importance for the performance of
346
materials.40 In this study, a stress-strain behaviour of electrospun fiber mat was
347
investigated by tensile test, and the corresponding data of tensile strength (TS),
348
Young's modulus (Y) and elongation at break (E) were calculated and shown in Figure
349
10. It can be seen that the obtained core-sheath electrosun fiber mat had a TS of 6.65
350
MPa, Y of 90.51 MPa and E of 132.3 %. TS accounts for the film mechanical
351
resistance due to the cohesion between the chains, Y indicates the stiff degree of film, 16
ACS Paragon Plus Environment
Page 16 of 46
Page 17 of 46
Journal of Agricultural and Food Chemistry
352
whereas E is a measure of toughness and stretch ability prior to breakage.41 For the
353
SA/PEO fiber mat, it was noted that the presence of PEO increased the TS and Y of SA
354
films, and as the ratio of PEO increased from 10% to 30%, the values of TS and Y
355
were enhanced from 2.97 MPa and 71.07 MPa to 4.45 MPa and 90.26 MPa,
356
respectively. Such a large increase in TS and Y could be attributed to the good
357
compatibility and also the formation of inter-molecular hydrogen bonds between the
358
hydroxyl groups of SA and oxygen atoms of PEO, which consequently restricts the
359
motion of the matrix and promotes rigidity. This observation was also supported by in
360
the FTIR and TG analysis. Similar phenomenon had been reported by Çaykara et al.35
361
Generally, an increase in TS is usually coupled with a decrease in E, however, no
362
significant decrease (P>0.5) on E was observed with the incorporation of PEO to SA in
363
spite of the increasing TS values in this study. This may be due to plasticizing effect of
364
the water absorbed and the plasticizer of F127 used.42 Regarding the CS/PVA system,
365
with the ratio of PVA increasing from 40% to 60%, TS and Y decreased from 8.37MPa
366
and 104.83 MPa to 7.28 MPa and 87.95 MPa, while E increased from 137.2 % to
367
171.5%, respectively. The reason was likely that CS had a high molecular weight and
368
hard backbones compared with PVA, similar results were also confirmed by Zhang et
369
al.43 Conversely, adding PVA into CS could greatly modify film’s flexibility and thus
370
leading to the increased E values, similar behavior was reported in other literature.44 It
371
had been reported that the mechanical property of composites can be affected by the
372
degree of crystallinity of the matrix,45 in this study, the good performance of tensile
373
strength, elongation, and modulus of obtained electrospun fiber mat can be associated 17
ACS Paragon Plus Environment
Journal of Agricultural and Food Chemistry
374
with its crystalline nature that demonstrated in XRD section.
375
Release profile and diffusion coefficient. In vitro release study was
376
performed to investigate the release profile of BSA from electrospun fiber mat
377
by mimicking mouth to colon transit. The results showed that a small percentage
378
of BSA (0.99), and the release exponent n was 1.043,
392
indicating the release mechanism was Super Case II transport, in which the
393
erosion of polymer matrix was dominant.18 This phenomenon was owing to the
394
gradual degradation of chitosan by β-glucosidase in SCF. Hence, it can be
18
ACS Paragon Plus Environment
Page 18 of 46
Page 19 of 46
Journal of Agricultural and Food Chemistry
395
concluded that the release of BSA from the fiber mat in SCF is a complex
396
process, in which the erosion was dominant.
397
Furthermore, the diffusion coefficients (D) of BSA from electrospun fiber mat in SGF,
398
SIF and SCF were also calculated. As described before, the release experimental data
399
can be divided into two regions: (1) the region of “short time” is valid for the first 60%
400
of the total released substance, and (2) the region of “long time” is corresponding to the
401
late state of release.23 Figure 11 showed the fitting curves of release data according to
402
equation 3 and 4, and the corresponding D values. It was noticed that the electrospun
403
fiber mat exhibited a lower D values in SGF and SIF. This can be attributed to the
404
alginate’s insolubility in SGF and the core component of chitosan that retarded BSA
405
release in SIF, hence, less amount of BSA would diffuse from the matrix. In SCF, larger
406
porosity was produced due to the degradation of chitosan by β-glucosidase, as respected,
407
a higher D was obtained. These data demonstrated that the degradation of matrix led to
408
the release of BSA, which was in accordance with the above research results that the
409
erosion was the dominant release mechanism.
410
Stability of BSA. Protein conformation plays an important role in determining the
411
bioactivity of protein. In this study, FTIR, a widely used technique for determining
412
secondary structure of protein, was applied to investigate the conformational changes
413
of BSA during the preparation of electrospun fiber mat. Common features of protein’s
414
FTIR spectra are the amide bands, among which, the amide I band (1700–1600 cm−1)
415
is the most useful one in the analysis of protein secondary structure.46 Generally, the
416
peaks between 1660 and 1650 cm−1 are considered to be characteristics of α-helical 19
ACS Paragon Plus Environment
Journal of Agricultural and Food Chemistry
417
structure; peaks range in 1640-1610 cm−1 represents β-sheet; the peaks at 1660-1700
418
cm−1 and 1640−1650 cm−1 are assigned to β-turns and random coil conformation,
419
respectively.46 By adding the peak areas assigned to particular secondary structure
420
elements, it was found that the native BSA contained 42.5% α-helix, 11.3% β-sheet,
421
21.4% β-turn and 24.8% random coil structures, suggesting that the secondary
422
structures of BSA were dominated by α-helix conformation
423
to the native BSA, the α-helix content of BSA that encapsulated in CS nanoparticle and
424
core-sheath electrospun fiber mat was decreased to be 38.6% and 36.8%, respectively,
425
while the β-sheets, turns, and random coil structures were all increased. It meant that a
426
part of α-helix was transformed into other second structures, which may be related to
427
the formation of intermolecular hydrogen bonding during the nanoparticle preparation.
428
Still, the encapsulated BSA was still regarded as native form according to the previous
429
definition.48 A similar reduction in the α-helix content of the released BSA from
430
nanoparticle was also observed by Kunda et al and Vakilian et al.49,50 Interestingly,
431
there was no significant difference in the α-helix content of BSA encapsulated in the
432
nanoparticle and fiber mat (P > 0.05), which was due to the protection of the
433
core-sheath structure of coaxial electrospinning. Yang et al also reported that the
434
core-sheath structured electrospun fibers protected the structural integrity of
435
encapsulated protein.51
47
(Figure 12). Compared
436
Besides FTIR, far-UV CD was also performed on the measurement of secondary
437
structure of BSA. As listed in Table 3, the control BSA contained 52.4% of α-helix, 8.7%
438
of β-strand, 15.9% of β-turn and 23.0% of random coil. The more content of α-helix 20
ACS Paragon Plus Environment
Page 20 of 46
Page 21 of 46
Journal of Agricultural and Food Chemistry
439
calculated from CD spectrum was owing to its sensitivity to α-helix. In line with the
440
aforementioned FTIR results, no significant difference in the α-helix content of BSA
441
encapsulated in the nanoparticle (47.6%) and fiber mat (46.1%) (P > 0.05). In
442
summary, FTIR and CD analysis clearly indicated that the encapsulated BSA in the
443
nanoparticle and electrospun fiber mat still kept their structural integrity, which was
444
favorable for the maintenance of protein bioactivity. The above results suggest that the
445
obtained electrospun fiber mat is a potential colon-specific controlled release delivery
446
system for bioactive protein and thus promising in functional foods.
447
ABBREVIATIONS USED
448
GIT, gastrointestinal tract; SA, sodium alginate; CS, chitosan; BSA, bovine serum
449
albumin; PEO, polyoxyethylene; PVA, polyvinyl alcohol; TPP, sodium
450
tripolyphosphate; SEM, scanning electron microscope; TEM,
451
transmission electron microscopy; AFM, atomic force microscope; CLSM, confocal
452
laser scanning microscopy; FTIR, fourier transform infrared spectroscopy; XRD,
453
X-Ray diffraction; TGA, thermogravimetric analysis; CD, circular dichroism; SGF,
454
simulated gastric fluid; SIF, simulated intestinal fluid; SCF, simulated colonic fluid.
455
ACKNOWLEDGEMENT
456
We acknowledge the National Natural Science Foundation of China (No.
457
31671852), the Natural Science Foundation of Guangdong Province (No.
458
2015A030313217), and the National Natural Science Foundation of China
459
(NSFC)-Guangdong Joint Foundation Key Project (No. U1501214) for financial
460
support. 21
ACS Paragon Plus Environment
Journal of Agricultural and Food Chemistry
461
REFERENCES
462
(1) Dias, M. I.; Ferreira, I. C. F. R.; Barreiro, M. F. Microencapsulation of bioactives
463
for food applications. Food Funct. 2015, 6 (4), 1035-1052.
464
(2) Ting, Y. W.; Zhao, Q.; Xia, C. X.; Huang, Q. R. Using in vitro and in vivo models
465
to evaluate the oral bioavailability of nutraceuticals. J. Agric. Food Chem. 2015, 63,
466
1332–1338.
467
(3) Pu H. Y.; Chen, L.; Li, X. X.; Xie, F. W.; Yu, L.; Li, L. An oral colon-targeting
468
controlled release system based on resistant starch acetate: synthetization,
469
characterization, and preparation of film-coating rellets. J. Agric. Food Chem. 2011, 59,
470
5738–5745.
471
(4) Renukuntla, J.; Vadlapudi, A. D.; Patel, A.; Boddu, S. H. S.; Mitra, A. K.
472
Approaches for enhancing oral bioavailability of peptides and proteins. Int. J. Pharm.
473
2013, 447, 75-93.
474
(5) Wu, Q. X.; Zhang, Q. L.; Lin, D. Q.; Yao, S. J. Characterization of novel lactoferrin
475
loaded capsules prepared with polyelectrolyte complexes. Int. J. Pharm. 2013, 455,
476
124-131.
477
(6) Cerchiara, T.; Abruzzo, A.; Parolin, C.; Vitali, B.; Bigucci, F.; Gallucci, M. C.;
478
Nicoletta, F. P.; Luppi, B. Microparticles based on chitosan/carboxymethylcellulose
479
polyelectrolyte complexes for colon delivery of vancomycin. Carbohydr. Polym. 2016,
480
143, 124-130.
481
(7) Kosaraju, S. L. Colon targeted delivery systems: review of polysaccharides for
482
encapsulation and delivery. Crit. Rev. Food Sci. Nutr. 2005, 45, 251-258. 22
ACS Paragon Plus Environment
Page 22 of 46
Page 23 of 46
Journal of Agricultural and Food Chemistry
483
(8) Situ, W. B.; Li, X. X.; Liu, J.; Chen, L. Preparation and characterization of
484
glycoprotein-resistant starch complex as a coating material for oral bioadhesive
485
microparticles for colon-targeted polypeptide delivery. J. Agric. Food Chem. 2015, 63,
486
4138–4147.
487
(9) Wen, P.; Zhu, D. H.; Wu, H.; Zong, M. H.; Jing, Y. R.; Han, S. Y. Encapsulation of
488
cinnamon essential oil in electrospun nanofibrous film for active food packaging. Food
489
Control 2016, 59, 366-376.
490
(10) Wen, P.; Feng, K.; Yang, H.; Huang, X.; Zong, M. H.; Lou, W. Y.; Li, N.; Wu, H.
491
Electrospun core-shell structured nanofilm as a novel colon-specific delivery system
492
for protein. Carbohydr. Polym. 2017, 169, 157-166.
493
(11) Wang, H. L.; Hao L. L.; Niu, B. C.; Jiang S. W.; Cheng, J. F.; Jiang, S. T. Kinetics
494
and antioxidant capacity of proanthocyanidins encapsulated in zein electrospun Fibers
495
by cyclic voltammetry. J. Agric. Food Chem. 2016, 64, 3083-3090.
496
(12) Aceituno-Medina, M.; Mendoza, S.; Rodríguez, B. A.; Lagaron, J. M.;
497
López-Rubio, A. Improved antioxidant capacity of quercetin and ferulic acid during
498
in-vitro digestion through encapsulation within food-grade electrospun fibers. J. Funct.
499
Foods 2015, 12, 332-341.
500
(13) Vigh, T.; Demuth, B.; Balogh, A.; Galata, D. L.; Van Assche, I.; Mackie, C.;
501
Vialpando, M.; Van Hove, B.; Psathas, P.; Borbas, E.; Pataki, H.; Boeykens, P.; Marosi,
502
G.; Verreck, G.; Nagy, Z. K. Oral bioavailability enhancement of flubendazole by
503
developing nanofibrous solid dosage forms. Drug Dev. Ind. Pharm. 2017, 1-8.
504
(14) Yang, G. Z.; Li, J. J.; Yu, D. G.; He, M. F.; Yang, J. H.; Williams, G. R. Nanosized 23
ACS Paragon Plus Environment
Journal of Agricultural and Food Chemistry
505
sustained-release drug depots fabricated using modified tri-axial electrospinning. Acta
506
Biomater. 2017, 53, 233-241.
507
(15) Wen, H. F.; Yang, C.; Yu, D. G.; Li, X. Y.; Zhang, D. F. Electrospun zein
508
nanoribbons for treatment of lead-contained wastewater. Chem. Eng. J. 2016, 290,
509
263-272.
510
(16) Yu, D. G.; Li, J. J.; Zhang, M.; Williams, G. R. High-quality Janus nanofibers
511
prepared using three-fluid electrospinning. Chem. Commun. 2017, 53 (33), 4542-4545.
512
(17) Jiang, H.; Wang, L.; Zhu, K. Coaxial electrospinning for encapsulation and
513
controlled release of fragile water-soluble bioactive agents. J. Controlled Release 2014,
514
193, 296-303.
515
(18) Wang, X.; Yu, D. G.; Li, X. Y.; Bligh, S. W. A.; Williams, G. R. Electrospun
516
medicated shellac nanofibers for colon-targeted drug delivery. Int. J. Pharm. 2015, 490,
517
384-390.
518
(19) Ghorani, B.; Tucker, N. Fundamentals of electrospinning as a novel delivery
519
vehicle for bioactive compounds in food nanotechnology. Food Hydrocolloids 2015,
520
51, 227-240.
521
(20) Wen, P.; Zhu, D. H.; Feng, K.; Liu, F. J.; Lou, W. Y.; Li, N.; Zong, M. H.; Wu, H.
522
Fabrication of electrospun polylactic acid nanofilm incorporating cinnamon essential
523
oil/β-cyclodextrin inclusion complex for antimicrobial packaging. Food Chem. 2016,
524
196, 996-1004.
525
(21) Noruzi, M. Electrospun nanofibres in agriculture and the food industry: a review.
526
J. Sci. Food Agric. 2016, 96 (14), 4663-4678. 24
ACS Paragon Plus Environment
Page 24 of 46
Page 25 of 46
Journal of Agricultural and Food Chemistry
527
(22) Gan, Q.; Wang, T. Chitosan nanoparticle as protein delivery carrier-Systematic
528
examination of fabrication conditions for efficient loading and release. Colloids Surf.,
529
B 2007, 59, 24-34.
530
(23) Krupa, I.; Nedelčev, T.; Chorvát Jr, D.; Račko, D.; Lacík, I. Glucose diffusivity
531
and porosity in silica hydrogel based on organofunctional silanes. Eur. Polym. J. 2011,
532
47, 1477-1484.
533
(24) Sreerama, N.; Woody, R. W. Estimation of protein secondary structure from
534
circular dichroism spectra: comparison of CONTIN, SELCON, and CDSSTR methods
535
with an expanded reference set. Anal. Biochem. 2000, 287, 252-260.
536
(25) Bonino, C. A.; Krebs, M. D.; Saquing, C. D.; Jeong, S. I.; Shearer, K. L.; Alsberg,
537
E.; Khan, S. A. Electrospinning alginate-based nanofibers: from blends to crosslinked
538
low molecular weight alginate-only systems. Carbohydr. Polym. 2011, 85, 111-119.
539
(26) Nie, H. R.; He, A. H.; Zheng, J. F.; Xu, S. S.; Li, J. X.; Han, C. C. Effects of
540
chain conformation and entanglement on the electrospinning of pure alginate.
541
Biomacromolecules 2008, 9, 1362-1365.
542
(27) Esnaashari, S. S.; Rezaei, S.; Mirzaei, E.; Afshari, H.; Rezayat, S. M.;
543
Faridi-Majidi, R. Preparation and characterization of kefiran electrospun nanofibers.
544
Int. J. Biol. Macromol. 2014, 70, 50-56.
545
(28) Koosha, M.; Mirzadeh, H. Electrospinning, mechanical properties, and cell
546
behavior study of chitosan/PVA nanofibers. J. Biomed. Mater. Res., Part A 2015, 103,
547
3081-3093.
548
(29) Jia, Y. T.; Gong, J.; Gu, X. H.; Kim, H. Y.; Dong, J.; Shen, X. Y. Fabrication and 25
ACS Paragon Plus Environment
Journal of Agricultural and Food Chemistry
549
characterization of poly (vinyl alcohol)/chitosan blend nanofibers produced by
550
electrospinning method. Carbohydr. Polym. 2007, 67 (3), 403-409.
551
(30) Cheng, M.; Deng, J.; Yang, F.; Gong, Y.; Zhao, N.; Zhang, X. Study on physical
552
properties and nerve cell affinity of composite films from chitosan and gelatin
553
solutions. Biomaterials 2003, 24 (17), 2871-2880.
554
(31) Yin, Y. J.; Yao, K. D.; Cheng, G. X.; Ma, J. B. Properties of polyelectrolyte
555
complex films of chitosan and gelatin. Polym. Int. 1999, 48 (6), 429-432.
556
(32) Yang, X.; Li, L.; Shang, S.; Tao, X. M. Synthesis and characterization of
557
layer-aligned poly(vinyl alcohol)/graphene nanocomposites. Polymer 2010, 51 (15),
558
3431-3435.
559
(33) Xu, X.; Jiang, L.; Zhou, Z.; Wu, X.; Wang, Y. Preparation and properties of
560
electrospun soy protein isolate/polyethylene oxide nanofiber membranes. ACS Appl.
561
Mater. Interfaces 2012, 4 (8), 4331-4337.
562
(34) Mruthyunjaya Swamy, T. M.; Ramaraj, B.; Siddaramaiah. Thermal and
563
morphological properties of SA/HPMC blends. J. Appl. Polym. Sci. 2009, 112,
564
2235-2240.
565
(35) Çaykara, T.; Demirci, S.; Eroğlu, M. S.; Güven, O. Poly(ethylene oxide) and its
566
blends with sodium alginate. Polymer 2005, 46, 10750-10757.
567
(36) Lewandowska, K. Miscibility and thermal stability of poly(vinyl alcohol)/chitosan
568
mixtures. Thermochim. Acta 2009, 493, 42-48.
569
(37) Chen, C. H.; Wang, F. Y.; Mao, C. F.; Liao, W. T.; Hsieh, C. D. Studies of
570
chitosan: II. preparation and characterization of chitosan/poly(vinyl alcohol)/gelatin 26
ACS Paragon Plus Environment
Page 26 of 46
Page 27 of 46
Journal of Agricultural and Food Chemistry
571
ternary blend films. Int. J. Biol. Macromol. 2008, 43, 37-42.
572
(38) Bonilla, J.; Fortunati, E.; Atarés, L.; Chiralt, A.; Kenny, J. M. Physical, structural
573
and antimicrobial properties of poly vinyl alcohol–chitosan biodegradable films. Food
574
Hydrocolloids 2014, 35, 463-470.
575
(39)
576
beta-chitin/poly(vinyl alcohol) blend films. Polym. Test. 2003, 22, 381-387.
577
(40) Lin, H. Y.; Chen, H. H.; Chang, S. H.; Ni, T. S. Pectin-chitosan-PVA nanofibrous
578
scaffold made by electrospinning and its potential use as a skin tissue scaffold. J.
579
Biomater. Sci., Polym. Ed. 2013, 24, 470-484.
580
(41) Silva, M. A. d.; Bierhalz, A. C. K.; Kieckbusch, T. G. Alginate and pectin
581
composite films crosslinked with Ca2+ ions: Effect of the plasticizer concentration.
582
Carbohydr. Polym. 2009, 77, 736-742.
583
(42) Duan, B.; Wu, L.; Yuan, X.; Hu, Z.; Li, X.; Zhang, Y.; Yao, K.; Wang, M. Hybrid
584
nanofibrous membranes of PLGA/chitosan fabricated via an electrospinning array. J.
585
Biomed. Mater. Res., Part A 2007, 83A, 868-878.
586
(43) Zhuang, P. Y.; Li, Y. L.; Fan, L.; Lin, J.; Hu, Q. L. Modification of chitosan
587
membrane with poly(vinyl alcohol) and biocompatibility evaluation. Int. J. Biol.
588
Macromol. 2012, 50, 658-663.
589
(44) Zhang, S.; Zou, Y.; Wei, T.; Mu, C.; Liu, X.; Tong, Z. Pervaporation dehydration
590
of binary and ternary mixtures of n-butyl acetate, n-butanol and water using PVA-CS
591
blended membranes. Sep. Purif. Technol. 2017, 173, 314-322.
592
(45) Mathew, A. P.; Oksman, K.; Sain, M., Mechanical properties of biodegradable
Peesan,
M.;
Rujiravanit,
R.;
Supaphol,
P.
27
ACS Paragon Plus Environment
Characterisation
of
Journal of Agricultural and Food Chemistry
593
composites from poly lactic acid (PLA) and microcrystalline cellulose (MCC). J. Appl.
594
Polym. Sci. 2005, 97 (5), 2014-2025.
595
(46) Peng, X.; Yao, D.; Pan, Y.; Yu, Q.; Ni, S.; Bian, H.; Huang, F.; Liang, H. Study on
596
the structural changes of bovine serum albumin with effects on polydatin binding by a
597
multitechnique approach. Spectrochim. Acta, Part A 2011, 81, 209-214.
598
(47) Yang, Y.; Feng, Y.; Wang, Y.; Wang, L.; Shi, W. Interactions between U(VI) and
599
bovine serum albumin. J. Radioanal. Nucl. Chem. 2013, 298, 903-908.
600
(48) Norde, W.; Giacomelli, C. E. BSA structural changes during homomolecular
601
exchange between the adsorbed and the dissolved states. J. Biotechnol. 2000, 79,
602
259-268.
603
(49) Kunda, N. K.; Alfagih, I. M.; Dennison, S. R.; Somavarapu, S.; Merchant, Z.;
604
Hutcheon, G. A.; Saleem, I. Y. Dry powder pulmonary delivery of cationic
605
PGA-co-PDL nanoparticles with surface adsorbed model protein. Int. J. Pharm. 2015,
606
492, 213-222.
607
(50) Vakilian, S.; Mashayekhan, S.; Shabani, I.; Khorashadizadeh, M.; Fallah, A.;
608
Soleimani, M. Structural stability and sustained release of protein from a multilayer
609
nanofiber/nanoparticle composite. Int. J. Biol. Macromol. 2015, 75, 248-257.
610
(51) Yang, Y.; Li, X.; Qi, M.; Zhou, S.; Weng, J. Release pattern and structural
611
integrity of lysozyme encapsulated in core–sheath structured poly(dl-lactide) ultrafine
612
fibers prepared by emulsion electrospinning. Eur. J. Pharm. Biopharm. 2008, 69,
613
106-116.
614 28
ACS Paragon Plus Environment
Page 28 of 46
Page 29 of 46
Journal of Agricultural and Food Chemistry
615
Figure captions
616
Figure 1. Effect of surfactant and mass ratio of SA to PEO on the fiber mat’s
617
morphology (other conditions: total polymer 8%, feed rate 0.25 mL/h, distance 15 cm,
618
voltage 18 kV)
619 620
Figure 2. Effect of the concentration of shell polymer on the fiber mat’s morphology
621
(other conditions: SA: PEO=80:20, feed rate 0.25 mL/h, distance 15 cm, voltage 18
622
kv)
623 624
Figure 3. Rheological properties of different shell solution. a) dynamical modulus
625
change and b) viscosity variation of shell solution with different concentration .
626 627
Figure 4. Effect of volume ratio of CS to PVA on the fiber mat’s morphology (other
628
conditions: feed rate 0.25 mL/h, distance 15 cm, voltage 18 kv)
629 630
Figure 5. AFM images of electrospun fiber mat (a) 2D, (b) 3D.
631 632
Figure 6. CLSM images of (a) shell layer labeled with FITC; (b) core layer labeled
633
with Rh B; (c) the merge of core-sheath nanofiber and TEM image (d) of electrospun
634
fiber mat.
635 636
Figure 7. FTIR spectra of different sample. 29
ACS Paragon Plus Environment
Journal of Agricultural and Food Chemistry
Page 30 of 46
637 638
Figure 8. X-ray diffraction patterns of different sample.
639 640
Figure 9. TG (a, c, e) and DTG (b, d, f) curves of different samples.
641 642
Figure 10. Tensile strength (a), Young’s modulus (b) and elongation at break (c)
643
curves of different sample (P1S9-PEO/SA (10:90); P2S8-PEO/SA (20:80);
644
P3S7-PEO/SA
645
P6C4-PVA/CS (60:40); CN-coaxial electrospun fiber mat).
(30:70);
P4C6-PVA/CS
(40:60);
P5C5-PVA/CS
(50:50);
646 647
Figure 11. The fitted curves and diffusion coefficients of BSA in different medium.
648 649
Figure 12. Secondary structure contents of different sample from deconvoluted
650
FTIR spectra. (1-native BSA, 2-BSA released from nanoparticle; 3-2-BSA released
651
from electrospun fiber mat).
652 653 654 655 656 657 658 30
ACS Paragon Plus Environment
Page 31 of 46
Journal of Agricultural and Food Chemistry
Table 1 Physical properties of electrospun solutions
659 Solution
SA
PEO
Surfactant and solvent Triton
F127
DMSO
Conductivity (mS/cm)
Viscosity (cP)
Surface tension (mN/m)
SA:PEO =90:10
8.1% 8.1% 8.1% 8.1%
0.9% 0.9% 0.9% 0.9%
0 1% 0 0
0 0 2% 2%
0 0 0 5%
11.34±0.22 a 11.12±0.077 a 11.02±0.23 a 9.22±0.040 b
2075.0±35.4 b 2079.0±29.7 b 2234.0±36.7 a 2352.0±128.6 a
52.688±0.164 a 33.224±0.0544 c 39.474±0.132 b 39.958±0.474 b
SA:PEO =80:20
7.2% 7.2% 7.2% 7.2%
1.8% 1.8% 1.8% 1.8%
0 1% 0 0
0 0 2% 2%
0 0 0 5%
10.04±0.18 a 9.89±0.11 a 9.45±0.10 b 8.01±0.060 c
2976.0±199.4 a 2996.5±45.8 a 3018.0±66.5 a 3140.0±63.6 a
49.886±0.515 a 33.501±0.159 c 39.351±0.255 b 39.278±0.295 b
SA:PEO =70:30
6.3% 6.3% 6.3% 6.3%
2.7% 2.7% 2.7% 2.7%
0 1% 0 0
0 0 2% 2%
0 0 0 5%
9.06±0.077 a 8.79±0.041 b 8.49±0.078 c 8.01±0.060 d
3656.5±284.9 b 3839.0±79.2 b 4700.0±141.4 a 3140.0±63.6 b
40.370±0.123 a 33.149±0.103 c 38.891±0.364 b 39.278±0.295 a
660 661 662 663
Note: different letters in the individual column of same mass ratio of SA to PEO indicate the significant difference (P