Study of Ni-Catalyzed Graphitization Process of Diamond by in Situ X

6 days ago - Graphene on diamond has been attracting considerable attention due to the unique and highly beneficial features of this heterostructure f...
0 downloads 7 Views 5MB Size
Subscriber access provided by - Access paid by the | UCSB Libraries

C: Surfaces, Interfaces, Porous Materials, and Catalysis

Study of Ni-catalyzed Graphitization Process of Diamond by In-situ X-ray Photoelectron Spectroscopy Oleksandr Romanyuk, Marian Varga, Semir Tulic, Tibor Izak, Petr Jiricek, Alexander Kromka, Viera Skakalova, and Bohuslav Rezek J. Phys. Chem. C, Just Accepted Manuscript • DOI: 10.1021/acs.jpcc.7b12334 • Publication Date (Web): 12 Mar 2018 Downloaded from http://pubs.acs.org on March 12, 2018

Just Accepted “Just Accepted” manuscripts have been peer-reviewed and accepted for publication. They are posted online prior to technical editing, formatting for publication and author proofing. The American Chemical Society provides “Just Accepted” as a service to the research community to expedite the dissemination of scientific material as soon as possible after acceptance. “Just Accepted” manuscripts appear in full in PDF format accompanied by an HTML abstract. “Just Accepted” manuscripts have been fully peer reviewed, but should not be considered the official version of record. They are citable by the Digital Object Identifier (DOI®). “Just Accepted” is an optional service offered to authors. Therefore, the “Just Accepted” Web site may not include all articles that will be published in the journal. After a manuscript is technically edited and formatted, it will be removed from the “Just Accepted” Web site and published as an ASAP article. Note that technical editing may introduce minor changes to the manuscript text and/or graphics which could affect content, and all legal disclaimers and ethical guidelines that apply to the journal pertain. ACS cannot be held responsible for errors or consequences arising from the use of information contained in these “Just Accepted” manuscripts.

is published by the American Chemical Society. 1155 Sixteenth Street N.W., Washington, DC 20036 Published by American Chemical Society. Copyright © American Chemical Society. However, no copyright claim is made to original U.S. Government works, or works produced by employees of any Commonwealth realm Crown government in the course of their duties.

Page 1 of 36 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

The Journal of Physical Chemistry

Study of Ni-catalyzed Graphitization Process of Diamond by In-situ Xray Photoelectron Spectroscopy

O. Romanyuk1,*, M. Varga1, S. Tulic2, T. Izak1, P. Jiricek1, A. Kromka1, V. Skakalova2, B. Rezek1,3

1

Institute of Physics, Academy of Sciences of the Czech Republic, Cukrovarnická 10, 162 00 Prague

6, Czech Republic

2

Physics of Nanostructured Materials, Faculty of Physics, University of Vienna, Boltzmanngasse 5,

1090 Vienna, Austria

3

Faculty of Electrical Engineering, Czech Technical University, Technická 2, Prague 6, Czech

Republic

*

Corresponding author. E-mail: [email protected]; tel.: +420 220 318 495

1 ACS Paragon Plus Environment

The Journal of Physical Chemistry 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 2 of 36

ABSTRACT: Graphene on diamond has been attracting considerable attention due to the unique and highly beneficial features of this heterostructure for a range of electronic applications. Here, ultra-high vacuum X-ray photoelectron spectroscopy is used for in-situ analysis of the temperature dependence of the Ni-assisted thermally-induced graphitization process of intrinsic nanocrystalline diamond thin films (65 nm thickness, 50-80 nm grain size) on silicon wafer substrates. Three major stages of diamond film transformation are determined from XPS during the thermal annealing in the temperature range from 300 °C to 800 °C. Heating from 300 °C causes removal of oxygen; formation of the disordered carbon phase is observed at 400 °C; the disordered carbon progressively transforms to graphitic phase whereas the diamond phase disappears from the surface from 500 °C. In the well controllable temperature regime between 600-700 °C, the nanocrystalline diamond thin film is mainly preserved, while graphitic layers form on the surface as the predominant carbon phase. Moreover, the graphitization is facilitated by a disordered carbon interlayer that inherently forms between diamond and graphitic layers by Ni catalyst. Thus, the process results in formation of a multilayer heterostructure on silicon substrate.

2 ACS Paragon Plus Environment

Page 3 of 36 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

The Journal of Physical Chemistry

INTRODUCTION

Many promising technological applications of graphene need high-quality large-scale sheets to be synthesized. There are various methods for large area graphene synthesis, such as thermally-induced growth on metal surfaces1,2, thermal, plasma chemical vapor deposition3–5, and thermal annealing of SiC surfaces6,7. For device production, subsequent exfoliation of the graphene sheet and graphene transfer procedures are required. These procedures, however, often lead to increased contamination and defects in graphene sheets. These undesired side effects can be detrimental for the performance of graphene-based devices. Direct fabrication of graphene-on-diamond heterostructures is now being explored as a promising alternative technology8. Graphene and diamond exhibit extraordinary intrinsic properties (thermal conductivity ~3000 J/Km and mechanical modulus ~1TPa) resulting from the C-C bonds which are related to the σ electronic states present in both crystal structures. In contrast, there is a significant difference in the electronic band structures of diamond and graphene due to the different electronic orbital hybridization – sp3 in diamond, and sp2 in graphene. While graphene behaves as a semimetal having a linear dispersion relation, diamond is a large bandgap semiconductor with high electrical resistivity in the intrinsic form. Combining these two materials and their complementary properties in a single system denoted as graphene-on-diamond is opening new prospects for fundamental science and for applications9–11. A straightforward method for making graphene-on-diamond is the simple transfer of CVDsynthesized graphene on to a diamond surface9. However, surface contamination by polymer residuals or acids cannot be completely avoided in this case12. Another way is directly to graphitize the topmost diamond surface by annealing at high temperatures and at low pressure. In the past, the graphitization process has mainly been studied on well-defined monocrystalline diamond surfaces. Graphitization on a bare monocrystalline diamond C(111) surface began at approximately 850 °C13, while for a bare monocrystalline diamond surface C(100) graphitization began at 1200 °C14. 3 ACS Paragon Plus Environment

The Journal of Physical Chemistry 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 4 of 36

Monocrystalline diamond substrates with a large surface area for graphene-on-diamond technology would be too costly for commercial applications. However, nanocrystalline diamond (NCD) offers an alternative, chemically-matched native platform for graphene synthesis. The growth technology for large-area NCD layers by CVD methods is well established15. Graphene formation on a diamond surface can be promoted by metal catalysts. Metals such as Ni, Cu or Fe are used to melt or dissolve carbon atoms16–19 and, therefore, to reduce the graphitization temperature of a diamond surface significantly. In particular, a graphitization temperature as low as 247 °C has been reported on Ni/C(100)14. Recently, graphene synthesis on an Ni / ultrananocrystalline diamond (UNCD) film by rapid thermal annealing (RTA) has been demonstrated8. The high-resolution C 1s spectrum measured on the graphene/UNCD surface was asymmetric. It was fitted by one (unspecified) function and assigned to the graphene-related component8. The photoelectron emission from the UNCD substrate and disordered carbon by Ni have not been considered. However, photoelectron emission from the layers below a few graphene layers is expected. Another recent papers dealt with Ni enhanced graphitization of amorphous carbon films (a-C) prepared by CVD20–22. The a-C/Ni films were annealed mainly in a hydrogen atmosphere. It was observed that carbon film exchanges with Ni film and graphitizes at elevated temperature23–25. Recent theoretical studies explained the graphitization mechanism for rapid thermal annealing: a-C to graphene transformation entails the metal-induced crystallization and layer exchange mechanism. Carbon dissolution in Ni was excluded26. In the present work, a detailed analysis of dynamic changes of carbon phases in an Ni / nanocrystalline diamond film with faceted diamond grains is carried out in-situ as a function of annealing temperatures up to 800 °C under ultrahigh vacuum (UHV) conditions, i.e. without a hydrogen atmosphere. We show that Ni-catalyzed graphitization considerably affects the NCD surface. X-ray photoelectron spectroscopy (XPS) data indicate a transformation of the diamond surface to disordered carbon at low temperatures and then, above 600 oC, to a graphitic/multilayer 4 ACS Paragon Plus Environment

Page 5 of 36 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

The Journal of Physical Chemistry

graphene phase covering the surface. Raman measurements confirm that diamond grains are preserved below the graphitized surface.

EXPERIMENTAL

NCD thin films (about 65 nm in thickness) were grown on p-type Si (100) substrates with a native oxide layer. Before the growth process, the Si substrates were ultrasonically cleaned in acetone, in isopropyl alcohol and were rinsed in deionized water. Then, the substrates were seeded by applying ultrasonic agitation in a nanodiamond colloid (NanoAmando aqueous dispersion of nanodiamond particles; concentration of the stock solution 5.0 w/v%; median nanodiamond size 4.8 ± 0.6 nm (98.8 wt%); dilution by deionized water 1:40 v:v). The diamond growth was performed by focused microwave plasma chemical vapor deposition (MW-CVD), using an ellipsoidal cavity resonator from a hydrogen and methane gas mixture (5% of CH4 in H2 atmosphere) at a total gas pressure of 6 kPa, microwave power of 3 kW and deposition time of 25 minutes. The substrate temperature was about 780 °C during the growth. As-grown NCD samples were transferred from the MW-CVD reactor to the metal evaporation chamber. A layer of 20 nm Ni was evaporated on top of the NCD films at room temperature. The Ni/NCD samples were then further transferred to the AXIS Supra X-ray photoelectron spectrometer (Kratos Analytical Ltd., UK). The Ni/NCD samples and the reference NCD sample were sequentially annealed and cooled down to room temperature in an analytical XPS chamber under ultra-high vacuum (UHV). The sample temperature was increased up to 800 oC in 100 oC steps in 20-30 minute intervals. The pressure in the XPS chamber was kept below 10-7 mbar during the XPS measurements. Survey XPS spectra and high-resolution C 1s, O 1s, and Ni 2p3/2 core level spectra were measured using monochromatized AlKα radiation (1486.6 eV, probe area is 0.7 × 0.3 mm2). Photoelectrons were collected in constant energy mode with a pass energy of 10 eV, resulting in overall energy 5 ACS Paragon Plus Environment

The Journal of Physical Chemistry 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 6 of 36

resolution of 0.45 eV, measured on the Ag 3d5/2 line width. The X-ray incidence angle was at 54.4o with respect to the surface normal, and XPS spectra were measured at the normal emission angle. All samples were sufficiently conductive, so charge compensation was not used during XPS spectra acquisition. The chemical composition of the film surface was determined from the corresponding photoelectron peak areas after standard Shirley inelastic background subtraction and using the relative sensitivity factor method. The high-energy resolution core level peaks were analyzed by peak fitting applying a few sets of lineshape functions: Doniach–Sunjic (DS) lineshapes27 convoluted with Gaussian functions were used as primary fit functions, and Voigt functions were used as a secondary set of functions in order to estimate the reliability of the DS fits. The two function sets provided similar results. As DS functions are more suitable for the analysis of graphite and graphene layers28,29, they are also preferred here. The shape of the DS function was derived independently by measuring the C 1s peak on cleaved highly oriented pyrolytic graphite (HOPG). A commercially available HOPG sample (MikroMasch company) was 10 x 10 x 1 mm3 in size and was of ZYB grade (mosaic spread: 0.8°). The HOPG sample was attached to the sample holder by two-sided scotch tape. In order to obtain a fresh, clean surface of the HOPG, the thin upper layer of the sample was removed using a razor blade just before the HOPG sample was inserted into the flexi-lock chamber of the photoelectron spectrometer. A negligible amount of oxygen contamination was confirmed on the freshly cleaved HOPG surface by XPS. The high-resolution C 1s experimental data and the corresponding fitted DS function are presented in Supporting information, Figure S1 and Table S1. The surface morphology of the diamond films was analyzed using Tescan MAIA3 field-emission scanning electron microscopy (SEM) equipped with an in-beam secondary electron detector. The thickness of the NCD film was evaluated from the interference fringes in the reflectance spectra measured in the range of 400 nm – 1000 nm.

6 ACS Paragon Plus Environment

Page 7 of 36 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

The Journal of Physical Chemistry

Raman spectra were measured using a Renishaw In Via Reflex Raman spectrometer with an excitation wavelength of 442 nm (He-Cd laser). The exposure time was set to 60 s, while the output power of the laser was decreased to 10% (~1 mW) to minimize the heating effect of the laser beam. All spectra were measured in a back-scattering setup with a 100x objective in the confocal mode with a grating of 2400 lines/mm and with a corresponding spectral resolution of 1.2 cm-1. The laser spot was approximately 5 µm in diameter.

RESULTS AND DISCUSSION

Figure 1a) shows a typical top-view SEM image of the as-grown NCD films30,31. The diamond grains are resolved. Grain sizes vary from of 50 – 80 nm. Figure 1b) shows that the evaporated 20 nm thick Ni layer conforms to the primary NCD surface morphology. Only the slightly smoothed grain edges and the homogenized secondary electron emission are noticeably different. Figures 1c) and 1d) show the representative surface morphology of the Ni/NCD sample after thermal annealing to 600 °C and 800 °C, respectively. There are black protrusions that have appeared in 1c), but the Ni/NCD film morphology is similar to the as-received Ni/NCD sample in 1b). The surface morphology becomes overall flatter and smoother in 1d): NCD grains are no longer recognized. Some crack-like dark features with bright edges appear on the film surface. The SEM features are corroborated by XPS analysis: XPS revealed no sp3 bond contributions of NCD grains on the annealed Ni/NCD surfaces. Figures 1e) and 1f) show 45°-view SEM images of the Ni/NCD annealed at 600 °C measured in secondary electron and back-scattered electron (BSE) modes, respectively. The SEM image [Figure 1e)] shows the surface morphology, whereas the SEM-BSE image [Figure 1f)] reveals the difference in the chemical composition on the same area. The Ni-contained layers and particles are the brightest, the pure carbon phases are the darkest and in between the composition of ‘C/Ni’ phases is present. This could be explained by additional carbon 7 ACS Paragon Plus Environment

The Journal of Physical Chemistry 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 8 of 36

layers on top of Ni layers. As will be shown later, the ‘C’ phase could correspond to the disordered or graphitic phase of carbon.

Figure 1. SEM secondary electron images of a) the as-grown NCD film b) the NCD film coated with a 20 nm Ni layer, c) the Ni/NCD sample annealed at 600 °C and d) annealed at 800 °C and cooled down to room temperature. SEM images of the partially delaminated region of the Ni/NCD annealed at 600 °C and measured under a 45° angle in e) secondary electron mode and f) in back-scattered electron mode.

8 ACS Paragon Plus Environment

Page 9 of 36 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

The Journal of Physical Chemistry

The dependence of the surface chemical composition on the annealing temperature was measured

in situ by XPS. It should be mentioned that the probe depth is limited due to photoelectron attenuation in solids. For the particular core level energies, the photoelectron inelastic mean free path is around 1.6 nm - 2.6 nm, which limits the photoelectron escape depth to about 3-7 nm. In addition, surface composition measurements can be affected by surface roughness, especially for angleresolved XPS32. We verified this effect on samples with different grain sizes. For normal photoelectron emission, however, the effect of surface roughness was found to be negligible. Figure 2a) shows the dependence of C, Ni, and O atomic concentrations on the annealing temperature obtained from the integrated core level XPS peak intensities. The as-prepared Ni/NCD film consisted of oxide layers on the surface. It is expected that the as-received Ni/NCD film is contaminated by O and Ni oxide layers, as the sample was exposed to air while it was being transferred to the XPS chamber. In our case, the O 1s core level peak involved two components, which are related to the C-O and Ni-O bonds (Figure S3 in Supporting information). Oxygen and Ni oxide almost disappeared from the Ni/NCD surface at 300 °C. The increase in Ni relative concentration up to about 68 at.% at 300 °C can therefore be attributed to the removal of surface contamination. In contrast to Ni, only a small decrease in carbon concentration is observed at 300 °C. The carbon signal must therefore mainly have originated from the NCD grains underneath the Ni thin film. The NCD surface is rough, and it could happen that the Ni coverage is not uniform on grain facets and grain boundaries or that there are cracks in the Ni layer.

9 ACS Paragon Plus Environment

The Journal of Physical Chemistry 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 10 of 36

Figure 2. a) Dependence of atomic compositions in the near-surface region of the samples on the annealing temperature obtained from the integrated core level XPS peak intensities. b) Dependence of the C 1s core level peak maxima on the annealing temperature. Cleaning, disordering and graphitization stages are marked by white, blue, and green colors of the background, respectively.

The Ni atomic concentration drops to less than 1.0 at.% at 700 °C (close to the detection limit of the XPS method), so Ni disappeared from the surface. As the temperature is too low for Ni evaporation (its melting point is 1455 °C), Ni atoms must be diffusing from the surface toward the bulk, as discussed below. At the same time, the carbon concentration at the surface increases steadily, and reaches 99 at.% at 700 °C. In Figure 2b), the C 1s peak maximum position moves from 285.4 eV at room temperature to a lower binding energy of 284.9 eV at 300 °C. Between 300 °C and 500 °C, the C 1s peak position moves back to higher binding energies. Finally, at a temperature of 500 °C the C 1s again moves back towards lower binding energies. The change in the C 1s peak position correlates with the changes in atomic concentrations on the surface (as indicated by the colored background). Peak shifts are caused by the formation of new carbon phases on the sample surface during the annealing process. 10 ACS Paragon Plus Environment

Page 11 of 36 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

The Journal of Physical Chemistry

Figure 3 shows the temperature dependence of high-resolution Ni 2p3/2 XPS spectra. XPS spectra below 300 °C (during oxygen desorption) are shown in Supporting information. Oxygen desorption33 up to T=300 °C did not have a crucial impact on graphitization. At temperatures above 300 oC, the Ni 2p3/2 peak position (852.9 eV) and the Ni energy loss peak position (858.8 eV) agree well with the corresponding energy position values for an Ni film prepared by sputtering33. At temperatures higher than 700 °C, the photoelectron emission from the Ni atoms dropped to the background level: the Ni atomic concentration decreased to less than 1 at.% on the sample surface, as shown in Figure 2a).

Figure 3. Ni 2p3/2 core level peak dependence on the annealing temperature measured on the Ni/NCD sample by XPS. The Ni 2p3/2 and Ni satellite peak position maxima, and also peak shapes do not depend on temperature. Peak intensity and, therefore, Ni concentration decrease with temperature, and they dropped to the background intensity level at 700 °C.

In contrast to the C 1s peak position maxima [Figure 2b)], the Ni 2p3/2 peak position maxima remain constant during annealing (Figure 3). In addition, the C-Ni peak components at low binding energies (283.3 eV)34,35 are not present on the C 1s spectra. These results have two fundamental 11 ACS Paragon Plus Environment

The Journal of Physical Chemistry 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 12 of 36

implications. Firstly, the shift of the C 1s peak position with temperature is not caused by band bending or by surface charge effects (the Ni peak position is constant). It must therefore be related to the change in the chemical state of the original diamond bonds at the surface. Hence, the phase transition takes place during the annealing process. Secondly, the XPS data confirm that Ni does not react chemically with carbon atoms, and indeed serves as a catalyst facilitating sp3 to sp2 carbon phase transformation at the diamond surface. Figure 4 elucidates this transformation by fitting the high-resolution C 1s core level peak measured on the Ni/NCD sample at different annealing temperatures (the C 1s spectra below 300 °C were not included here, since a study of oxide desorption is beyond the scope of the present paper). The C1s peak positions, the peak component widths and the asymmetry factors of DS functions for all annealing stages are given in Supporting information (Table S1). The fluctuation in binding energy of ±0.1 eV is possibly due to a finite data acquisition energy step of 0.1 eV and due to the error bar of the fitting procedure.

12 ACS Paragon Plus Environment

Page 13 of 36 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

The Journal of Physical Chemistry

Figure 4. Temperature dependence of the high-resolution C 1s core level peaks measured on the Ni/NCD surface by XPS. The experimental data are marked by dots, the fitted spectra are marked by solid black lines, and the component envelopes are marked by filled color lines. The C 1s peaks consist of sp3 (red) and sp2 (blue) components of the NCD substrate at 300 oC and at 400 oC; disordered carbon (Cdis, cyan) is present at 400 oC; the graphitic phase component (G, green) appears at T>500 oC. The concentration of the graphitic phase is indicated as a relative %.

13 ACS Paragon Plus Environment

The Journal of Physical Chemistry 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 14 of 36

The C 1s peak at 300 °C and 400 °C involves a dominant sp3 component and a few percent of sp2 component. The sp3 peak position (284.9 eV) and the sp2 peak position (283.8 eV) agree well with the corresponding values of the C 1s core level peak positions for an NCD surface36. It should be emphasized, however, that the C 1s peak position maxima can vary for different forms of carbon with different types of bond hybridization, surface contamination (C-O bond concentration), or with the surface charge effect (especially for an undoped semiconductor). The sp3 to sp2 component energy difference of around 0.9 – 1.1 eV (as also observed here) is thus a more reliable characteristic of NCD films36. A few percent of oxygen still remains on the surface after annealing at 300 °C [see also Figure 2a)], but most of the photoelectrons originate from the NCD film at this temperature. The C 1s peak maximum is shifted to the direction of higher binding energy between 400 °C – 600 °

C. The shift is caused by the Cdis component at 285.2 eV. At higher temperatures (T > 700 °C),

another G component at 284.8 eV is responsible for the C 1s peak maxima shift backward to lower binding energies. Since the C 1s binding energy positions vary in the literature for different carbon phases and experimental conditions, it is not straightforward to identify the particular component. In order to identify the components, component peak shape analysis (asymmetry of the peak) and Raman measurements of the annealed Ni/NCD samples were carried out. Typically, symmetric Gaussian or Lorentzian functions, or a combination of them, are used for deconvolution of high-resolution C 1s spectra measured on NCD, on diamond-like carbon (DLC) or on amorphous carbon films. The C 1s peak of clean, contamination-free conductive carbon films such as HOPG, graphene or graphitic films is asymmetric28. In this case, the asymmetry of the C 1s peak is related to the shake-off photoelectron effects29, and an asymmetric function seems to be more appropriate for C 1s spectrum deconvolution. Our fit revealed asymmetry of the high-resolution C 1s spectra for both the reference HOPG sample (α = 0.09 in DS function) and the G component of the annealed Ni/NCD sample (α = 0.10 0.12). It should be emphasized that, for temperatures higher than 400 °C, there would be no oxygen contamination on the Ni/NCD samples, and the spectra asymmetry is not due to oxygen bond 14 ACS Paragon Plus Environment

Page 15 of 36 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

The Journal of Physical Chemistry

contributions. In addition, the π-plasmon peak37,38, which is typical for graphitic/graphene layers, was measured on both the HOPG sample and the Ni/NCD sample annealed at high temperatures (see Supporting information). Therefore, a dominant asymmetric component of the C 1s peak at 284.8 eV was identified as originating from graphitic (G) layers. The presence of graphitic layers on the Ni/NCD samples annealed at high temperature was also confirmed by Raman measurements, as discussed below. In contrast to the G components, the Cdis components at 285.2 eV are symmetric (α = 0.0) and πplasmons were absent in C 1s spectra up to 600 °C. This component was attributed to the disordered carbon (also supported by the D-band peak in the Raman spectra below). A similar energy difference of 0.4 eV between the graphene component (Gr) and the ‘deleterious’ phase of carbon (CB) has been measured previously during graphene growth on Ni by the CVD method39. The CB component has been identified as an sp3-related component, which is questionable since no diamond (sp3) peak is present in the Raman spectra there. However, the CB component can be correlated with the D-band peak in the Raman spectra39 similar to our case, and the CB component is related to disordered carbon, rather than to the diamond. Our XPS measurements therefore confirm that Ni amorphizes the NCD surface during its diffusion into the NCD film, i.e. disordering by Ni catalysis occurs prior to surface graphitization. The disordered carbon phase concentration further increases with respect to the NCD phase concentration with increasing temperature. At 500 °C, the C 1s peak consists of a dominant Cdis component, whereas the sp3 and sp2 components of the NCD films are absent although some NCD areas can be seen rarely on SEM images close to defects (the NCD fraction is below the detection limit of XPS). Therefore, Ni amorphizes the NCD film drastically, rather than ‘gently’ diffusing into the NCD film through its grain boundaries. In addition to the disordered carbon peak component, the G component at 284.8 eV appears at 500 °C. This temperature seems to be crucial for graphitic layer formation on a disordered NCD surface. The concentration of the graphitic phase, i.e. the area of the G component, further increases with increasing annealing temperature up to 700 oC. 15 ACS Paragon Plus Environment

The Journal of Physical Chemistry 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 16 of 36

The position of the G component at 284.8 eV is somewhat different from the position of the graphene component at 284.4 eV in the literature12,39, but it is closer to the corresponding C 1s peak position of 284.6 eV measured here on HOPG (see Supporting information) and on graphene/UNCD8. In addition, the full width at half maxima (FWHM) of the G component and the asymmetry factors are quite similar to the corresponding parameters of the C 1s peak measured on HOPG. The 0.2 eV difference in G peak position could therefore be related to the quality of the film or to the number of graphene/graphitic layers. In Figure 5, the sp2/sp3 component area ratio (red spheres) and the G/Cdis component area ratio (green squares) are shown as a function of the annealing temperature. At lower annealing temperatures, 6% of the sp2 bonds and 92% of the sp3 bonds were derived on the Ni/NCD surface (the ratio is 0.06). The disordered carbon phase concentration is higher than the graphitic phase concentration up to 600 °C. At temperatures of 700 °C and higher, the ratio G/Cdis is greater than 1, indicating graphitization of the disordered phase on the surface. When the sample is cooled back to room temperature, the G/Cdis ratio decreases slightly, most likely due to re-ordering of carbon atoms on the surface. In any case, the coexistence of graphitic and disordered carbon phases is well recognized on the surface.

Figure 5. Temperature dependence of graphitic-to-diamond (or graphitic-to-disordered) peak component ratios. The graphitic phase concentration increased steeply at 700 oC. The error bars were estimated from two different fits with the use of DS and Voigt functions. The disordered phase concentration rose slightly when the sample was cooled down to room temperature (RT). 16 ACS Paragon Plus Environment

Page 17 of 36 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

The Journal of Physical Chemistry

In summary, XPS analysis confirmed the formation of disordered and graphitic layers on Ni/NCD surface at T>500 °C. This finding can be correlated with SEM observations. In Figs. 1c), 1e), and 1f), a new carbon phase, ‘C’, is present which could be related to the disordered and/or graphitic phase according to XPS measurements (see Cdis and G components in C 1s spectra). The ‘C/Ni’ phase covered the sample surface almost completely at T=600 °C and only a few spots of pure ‘C’ phase were present. Since the atomic concentration of Ni was about 30 at.% only for T=600 °C [Figure 2a)], the ‘C/Ni’ phase thus corresponds to the Ni layers covered by carbon phases. In other words, melted disordered carbon atoms have to diffuse from the Ni/NCD interface upward to the Ni surface. Figure 6 shows Raman spectra of the reference NCD sample annealed at 800 oC (without Ni) and the Ni/NCD samples annealed at 600 oC and 800 oC. For the reference NCD sample (red curve), there are two dominant peaks: a sharp diamond-peak at 1331 cm-1, which is attributed to diamond bonds, and a broad band at ~1560 cm-1 (a mixture of sp3 / sp2 carbon bonds). In addition, there is a small band at 1150 cm-1, which is characteristic for NCD, and it is attributed to trans-polyacetylenelike groups40. The Raman spectrum of the as-grown NCD, i.e. before annealing, is not shown here, as it is similar to the Raman spectrum of the reference annealed NCD sample. Thus, the bare NCD film is rather stable during annealing up to 800 oC in UHV.

17 ACS Paragon Plus Environment

The Journal of Physical Chemistry 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 18 of 36

Figure 6. Raman spectra of the annealed reference NCD sample (T=800 oC, red curve) and the annealed Ni/NCD sample (T=600 oC, green curve, and T=800 oC, black curve). The Ni/NCD spectra contain an additional D-band due to the disordered carbon phase, and G-, 2D-bands due to the graphitic phase. In contrast to the reference NCD Raman spectrum (Figure 6, red curve), the spectrum of the annealed Ni/NCD at 600 °C contains an additional so-called D-band (defect-band) peak at 1370 cm-1 and a small G-band (graphitic) peak41,42 at 1582 cm-1 (Figure 6, green curve). The D-band peak is related to a disordered carbon phase and G-band is related to a graphitic phase. It agrees with the XPS findings of the Cdis and G components of the C 1s peak. The D-band peak intensity is enhanced relative to the diamond peak intensity at a higher temperature (black curve, 800 oC). Therefore, more defects in NCD are present at higher annealing temperatures. In addition, the sharp graphite G-band at 1582 cm-1 and the 2D-band at 2740 cm-1 are present in the Raman spectrum at 800 oC. A diamond-peak is also observed at 1331 cm-1, reflecting the presence of retained NCD grains. Its intensity is lower than in the G-band and 2D-band peaks, however. The intensity ratio of 2D/G is about 0.5, which corresponds to multilayered graphene or thick graphitic layers, rather than to a single graphene layer8. It should be noted that the underlying 18 ACS Paragon Plus Environment

Page 19 of 36 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

The Journal of Physical Chemistry

NCD film was not measured by XPS, due to the limited escape depth of the photoelectrons. In the case of Raman measurements, the probe depth is significantly larger and an NCD film was clearly observed beneath the graphitic phase. Thus, a sequence of carbon phase transformations during the Ni-catalytic reaction on the Ni/NCD samples was identified by Raman measurements. The D-band appears prior to the G- and 2D-bands during annealing, which is in line with in situ XPS results. A schematic diagram of the annealing process is shown in Figure 7. The Ni layer becomes free of oxide and contaminations at temperatures higher than 300 °C [Figure 7a)]. The Ni layers melt the NCD film at the Ni/NCD interface and disordered carbon diffuses onto the Ni layer surface [Figure 7b)]. A layer exchange mechanism of this kind was also observed for amorphous carbon/Ni heterostructures23–25. Then the graphitic layers are formed at T>500 °C [Figure 7c)] according to results observed from XPS measurements. Finally, the graphitic phase concentration increases with the annealing temperature (T>700 °C), and its concentration became higher than the concentration of the disordered phase [Figure 7d)]. According to Raman measurements, the NCD film was partially preserved and according to the XPS measurements the Ni film disappeared from the surface and thus has to be embedded beneath the surface carbon layer.

Figure 7. Schematic diagram of the Ni-catalyzed graphitization process on an NCD film. The oxygen free Ni film (a) melts the NCD film in b). Disordered carbon diffuses on the Ni surface and partially graphitizes in c). Disordered carbon recrystallizes to graphitic phase at a high annealing temperature (d). 19 ACS Paragon Plus Environment

The Journal of Physical Chemistry 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 20 of 36

CONCLUSIONS

Step-by-step graphitization of an NCD thin film surface was thermally induced by Ni-catalyzed reactions and was investigated in-situ by XPS. Several phase transitions during thermal annealing were revealed. Deconvolution and a detailed analysis of the high-resolution C 1s spectra measured during the annealing process revealed disordering of the NCD surface above 300 oC. Graphitization starts at 500 oC and the graphitic-to-disordered C phase ratio increases with increasing temperature. At 700 oC, the fraction of the graphitic phase became about two times higher than the fraction of the disordered C phase. Diamond was not preserved on the surface (i.e. within the 3-5 nm escape depth of the photoelectrons), while the Raman spectra still confirmed the presence of underlying NCD grains. Thus, a graphitic / disordered carbon / NCD multilayer structure had been formed. The data that have been obtained open attractive perspectives for controllable graphitization of diamond surfaces and for the synthesis of graphene or graphene heterostructures on wafer scale.

ACKNOWLEDGMENTS

Financial support from the Czech Science Foundation (project number 16-34856L) and from the Austrian Science Foundation (project number 2344-N36) is gratefully acknowledged. We acknowledge support from the Ministry of Education, Youth and Sports of the Czech Republic (MSMT project LM2015087). All authors thank Dr. K. Hruška, Dr. T. Susi, Kateřina Dragounová and Prof. T. Waitz for their assistance and for fruitful discussions.

Supporting Information Available: the C 1s peak measured on a freshly cleaved HOPG sample and fitted with the Doniach-Sunjic (DS) asymmetric function; a list of fitting parameters of the C 1s peaks; the energy loss spectra close to the C 1s peak measured on the reference NCD sample and on

20 ACS Paragon Plus Environment

Page 21 of 36 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

The Journal of Physical Chemistry

the annealed Ni/NCD sample; the Ni 2p3/2 and O 1s core level peaks of Ni/NCD sample. This material is available free of charge via the Internet at http://pubs.acs.org

REFERENCES

(1) (2) (3)

(4)

(5)

(6)

(7) (8)

(9) (10)

(11) (12) (13)

(14) (15) (16)

Edwards, R. S.; Coleman, K. S. Graphene Film Growth on Polycrystalline Metals. Acc. Chem. Res. 2013, 46, 23–30. Voloshina, E.; Dedkov, Y. Graphene on Metallic Surfaces: Problems and Perspectives. Phys. Chem. Chem. Phys. 2012, 14, 13502. Hawaldar, R.; Merino, P.; Correia, M. R.; Bdikin, I.; Grácio, J.; Méndez, J.; Martín-Gago, J. A.; Singh, M. K. Large-Area High-Throughput Synthesis of Monolayer Graphene Sheet by Hot Filament Thermal Chemical Vapor Deposition. Sci. Rep. 2012, 2, 1–9. Li, X.; Cai, W.; An, J.; Kim, S.; Nah, J.; Yang, D.; Piner, R.; Velamakanni, A.; Jung, I.; Tutuc, E.; et al. Large-Area Synthesis of High-Quality and Uniform Graphene Films on Copper Foils. Science 2009, 324, 1312–1314. Yamada, T.; Ishihara, M.; Kim, J.; Hasegawa, M.; Iijima, S. A Roll-to-Roll Microwave Plasma Chemical Vapor Deposition Process for the Production of 294mm Width Graphene Films at Low Temperature. Carbon 2012, 50, 2615–2619. Berger, C.; Song, Z.; Li, T.; Li, X.; Ogbazghi, A. Y.; Feng, R.; Dai, Z.; Marchenkov, A. N.; Conrad, E. H.; First, P. N.; et al. Ultrathin Epitaxial Graphite: 2D Electron Gas Properties and a Route toward Graphene-Based Nanoelectronics. J. Phys. Chem. B 2004, 108, 19912–19916. Starke, U.; Riedl, C. Epitaxial Graphene on SiC(0001) and SiC(000-1): From Surface Reconstructions to Carbon Electronics. J. Phys. Condens. Matter 2009, 21, 134016. Berman, D.; Deshmukh, S. A.; Narayanan, B.; Sankaranarayanan, S. K. R. S.; Yan, Z.; Balandin, A. A.; Zinovev, A.; Rosenmann, D.; Sumant, A. V. Metal-Induced Rapid Transformation of Diamond into Single and Multilayer Graphene on Wafer Scale. Nat. Commun. 2016, 7, 12099. Wu, Y.; Lin, Y.; Bol, A. A.; Jenkins, K. A.; Xia, F.; Farmer, D. B.; Zhu, Y.; Avouris, P. HighFrequency, Scaled Graphene Transistors on Diamond-like Carbon. Nature 2011, 472, 74–78. Yu, J.; Liu, G.; Sumant, A. V.; Goyal, V.; Balandin, A. A. Graphene-on-Diamond Devices with Increased Current-Carrying Capacity: Carbon Sp2-on-Sp3 Technology. Nano Lett. 2012, 12, 1603–1608. Wang, Y.; Jaiswal, M.; Lin, M.; Saha, S.; Özyilmaz, B.; Loh, K. P. Electronic Properties of Nanodiamond Decorated Graphene. ACS Nano 2012, 6, 1018–1025. Lin, Y.-C.; Lu, C.-C.; Yeh, C.-H.; Jin, C.; Suenaga, K.; Chiu, P.-W. Graphene Annealing: How Clean Can It Be? Nano Lett. 2012, 12, 414–419. Ogawa, S.; Yamada, T.; Ishizduka, S.; Yoshigoe, A.; Hasegawa, M.; Teraoka, Y.; Takakuwa, Y. Vacuum Annealing Formation of Graphene on Diamond C(111) Surfaces Studied by RealTime Photoelectron Spectroscopy. Jpn. J. Appl. Phys. 2012, 51, 11PF02. Pitter, M.; Hugenschmidt, M. B.; Behm, R. J. The Nickel/Diamond(100)–(2 × 1)H Interface Studied with Electron Spectroscopy. Jpn. J. Appl. Phys. 1997, 36, 3635–3638. Kromka, A.; Babchenko, O.; Izak, T.; Hruska, K.; Rezek, B. Linear Antenna Microwave Plasma CVD Deposition of Diamond Films over Large Areas. Vacuum 2012, 86, 776–779. Amini, S.; Garay, J.; Liu, G.; Balandin, A. A.; Abbaschian, R. Growth of Large-Area Graphene Films from Metal-Carbon Melts. J. Appl. Phys. 2010, 108, 094321.

21 ACS Paragon Plus Environment

The Journal of Physical Chemistry 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 22 of 36

(17) Kanada, S.; Nagai, M.; Ito, S.; Matsumoto, T.; Ogura, M.; Takeuchi, D.; Yamasaki, S.; Inokuma, T.; Tokuda, N. Fabrication of Graphene on Atomically Flat Diamond (111) Surfaces Using Nickel as a Catalyst. Diam. Relat. Mater. 2017, 75, 105–109. (18) Huang, L.; Chang, Q. H.; Guo, G. L.; Liu, Y.; Xie, Y. Q.; Wang, T.; Ling, B.; Yang, H. F. Synthesis of High-Quality Graphene Films on Nickel Foils by Rapid Thermal Chemical Vapor Deposition. Carbon 2012, 50, 551–556. (19) García, J. M.; He, R.; Jiang, M. P.; Kim, P.; Pfeiffer, L. N.; Pinczuk, A. Multilayer Graphene Grown by Precipitation upon Cooling of Nickel on Diamond. Carbon 2011, 49, 1006–1012. (20) Saenger, K. L.; Tsang, J. C.; Bol, A. A.; Chu, J. O.; Grill, A.; Lavoie, C. In Situ X-Ray Diffraction Study of Graphitic Carbon Formed during Heating and Cooling of AmorphousC/Ni Bilayers. Appl. Phys. Lett. 2010, 96, 153105. (21) Kwak, J.; Chu, J. H.; Choi, J.-K.; Park, S.-D.; Go, H.; Kim, S. Y.; Park, K.; Kim, S.-D.; Kim, Y.-W.; Yoon, E.; et al. Near Room-Temperature Synthesis of Transfer-Free Graphene Films. Nat. Commun. 2012, 3, 1–7. (22) Wenisch, R.; Hübner, R.; Munnik, F.; Melkhanova, S.; Gemming, S.; Abrasonis, G.; Krause, M. Nickel-Enhanced Graphitic Ordering of Carbon Ad-Atoms during Physical Vapor Deposition. Carbon 2016, 100, 656–663. (23) Murata, H.; Toko, K.; Saitoh, N.; Yoshizawa, N.; Suemasu, T. Direct Synthesis of Multilayer Graphene on an Insulator by Ni-Induced Layer Exchange Growth of Amorphous Carbon. Appl. Phys. Lett. 2017, 110, 033108. (24) Janke, D.; Hulman, M.; Wenisch, R.; Gemming, S.; Rafaja, D.; Krause, M. Influence of Nickel Catalyst Morphology on Layer-Exchange-Based Carbon Crystallisation of Ni/a-C Bilayers. Phys. Status Solidi B 2017, 254, 1700234. (25) Murata, H.; Saitoh, N.; Yoshizawa, N.; Suemasu, T.; Toko, K. High-Quality Multilayer Graphene on an Insulator Formed by Diffusion Controlled Ni-Induced Layer Exchange. Appl. Phys. Lett. 2017, 111, 243104. (26) Chen, S.; Xiong, W.; Zhou, Y. S.; Lu, Y. F.; Zeng, X. C. An Ab Initio Study of the NickelCatalyzed Transformation of Amorphous Carbon into Graphene in Rapid Thermal Processing. Nanoscale 2016, 8, 9746–9755. (27) Doniach, S.; Sunjic, M. Many-Electron Singularity in X-Ray Photoemission and X-Ray Line Spectra from Metals. J. Phys. C Solid State Phys. 1970, 3, 285–291. (28) Hunt, M. R. C. Surface and Bulk Components in Angle-Resolved Core-Level Photoemission Spectroscopy of Graphite. Phys. Rev. B 2008, 78, 153408. (29) Susi, T.; Pichler, T.; Ayala, P. X-Ray Photoelectron Spectroscopy of Graphitic Carbon Nanomaterials Doped with Heteroatoms. Beilstein J. Nanotechnol. 2015, 6, 177–192. (30) Kozak, H.; Kromka, A.; Ukraintsev, E.; Houdkova, J.; Ledinsky, M.; Vaněček, M.; Rezek, B. Detecting Sp2 Phase on Diamond Surfaces by Atomic Force Microscopy Phase Imaging and Its Effects on Surface Conductivity. Diam. Relat. Mater. 2009, 18, 722–725. (31) Kozak, H.; Remes, Z.; Kromka, A.; Ledinsky, M. Optical Characterisation of OrganosilaneModified Nanocrystalline Diamond Films. Chem. Pap. 2011, 65, 36–41. (32) Olejnik, K.; Zemek, J.; Werner, W. S. M. Angular-Resolved Photoelectron Spectroscopy of Corrugated Surfaces. Surf. Sci. 2005, 595, 212–222. (33) Kim, K. S.; Winograd, N. X-Ray Photoelectron Spectroscopic Studies of Nickel-Oxygen Surfaces Using Oxygen and Argon Ion-Bombardment. Surf. Sci. 1974, 43, 625–643. (34) Furlan, A.; Lu, J.; Hultman, L.; Jansson, U.; Magnuson, M. Crystallization Characteristics and Chemical Bonding Properties of Nickel Carbide Thin Film Nanocomposites. J. Phys. Condens. Matter 2014, 26, 415501. (35) Wiltner, A.; Linsmeier, C. Formation of Endothermic Carbides on Iron and Nickel. Phys. Status Solidi A 2004, 201, 881–887. (36) Chu, P. K.; Li, L. Characterization of Amorphous and Nanocrystalline Carbon Films. Mater. Chem. Phys. 2006, 96, 253–277. 22 ACS Paragon Plus Environment

Page 23 of 36 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

The Journal of Physical Chemistry

(37) Butenko, Y. V.; Krishnamurthy, S.; Chakraborty, A. K.; Kuznetsov, V. L.; Dhanak, V. R.; Hunt, M. R. C.; Šiller, L. Photoemission Study of Onionlike Carbons Produced by Annealing Nanodiamonds. Phys. Rev. B 2005, 71, 075420. (38) Fink, J.; Müller-Heinzerling, T.; Pflüger, J.; Scheerer, B.; Dischler, B.; Koidl, P.; Bubenzer, A.; Sah, R. E. Investigation of Hydrocarbon-Plasma-Generated Carbon Films by ElectronEnergy-Loss Spectroscopy. Phys. Rev. B 1984, 30, 4713–4718. (39) Weatherup, R. S.; Bayer, B. C.; Blume, R.; Baehtz, C.; Kidambi, P. R.; Fouquet, M.; Wirth, C. T.; Schlögl, R.; Hofmann, S. On the Mechanisms of Ni-Catalysed Graphene Chemical Vapour Deposition. ChemPhysChem 2012, 13, 2544–2549. (40) Pfeiffer, R.; Kuzmany, H.; Salk, N.; Günther, B. Evidence for Trans-Polyacetylene in Nanocrystalline Diamond Films from H–D Isotropic Substitution Experiments. Appl. Phys. Lett. 2003, 82, 4149–4150. (41) Ferrari, A. C. Raman Spectroscopy of Graphene and Graphite: Disorder, Electron–phonon Coupling, Doping and Nonadiabatic Effects. Solid State Commun. 2007, 143, 47–57. (42) Malard, L. M.; Pimenta, M. A.; Dresselhaus, G.; Dresselhaus, M. S. Raman Spectroscopy in Graphene. Phys. Rep. 2009, 473, 51–87.

23 ACS Paragon Plus Environment

The Journal of Physical Chemistry 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 24 of 36

TOC Graphic

24 ACS Paragon Plus Environment

Page 25 of 36 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

The Journal of Physical Chemistry

25 ACS Paragon Plus Environment

The Journal of Physical Chemistry 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 26 of 36

26 ACS Paragon Plus Environment

Page 27 of 36 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

The Journal of Physical Chemistry

27 ACS Paragon Plus Environment

The Journal of Physical Chemistry 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 28 of 36

28 ACS Paragon Plus Environment

Page 29 of 36 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35

The Journal of Physical Chemistry

ACS Paragon Plus Environment

The Journal of Physical Chemistry 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

ACS Paragon Plus Environment

Page 30 of 36

Page 31 of 36

The Journal of Physical Chemistry

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

ACS Paragon Plus Environment

The Journal of Physical Chemistry 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

ACS Paragon Plus Environment

Page 32 of 36

Page 33 of 36

The Journal of Physical Chemistry

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

ACS Paragon Plus Environment

The Journal of Physical Chemistry 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47

ACS Paragon Plus Environment

Page 34 of 36

Page 35 of 36

The Journal of Physical Chemistry

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

ACS Paragon Plus Environment

The Journal of Physical Chemistry 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

ACS Paragon Plus Environment

Page 36 of 36