Sulfonated Terpolymers Containing Alkylene and ... - ACS Publications

39. 40. 41. 42. 43. 44. 45. 46. 47. 48. 49. 50. 51. 52. 53. 54. 55. 56. 57. 58. 59. 60 ... controlled to be m/n = 0.5/0.5 for SPA-A, 0.65/0.35 for SPA...
1 downloads 0 Views 1MB Size
Subscriber access provided by University of Winnipeg Library

Article

Sulfonated Terpolymers Containing Alkylene and Perfluoroalkylene Groups: Effect of Aliphatic Groups on Membrane Properties and Interface with the Catalyst Layers Jinju Ahn, and Kenji Miyatake ACS Appl. Energy Mater., Just Accepted Manuscript • DOI: 10.1021/acsaem.8b00684 • Publication Date (Web): 11 Jul 2018 Downloaded from http://pubs.acs.org on July 11, 2018

Just Accepted “Just Accepted” manuscripts have been peer-reviewed and accepted for publication. They are posted online prior to technical editing, formatting for publication and author proofing. The American Chemical Society provides “Just Accepted” as a service to the research community to expedite the dissemination of scientific material as soon as possible after acceptance. “Just Accepted” manuscripts appear in full in PDF format accompanied by an HTML abstract. “Just Accepted” manuscripts have been fully peer reviewed, but should not be considered the official version of record. They are citable by the Digital Object Identifier (DOI®). “Just Accepted” is an optional service offered to authors. Therefore, the “Just Accepted” Web site may not include all articles that will be published in the journal. After a manuscript is technically edited and formatted, it will be removed from the “Just Accepted” Web site and published as an ASAP article. Note that technical editing may introduce minor changes to the manuscript text and/or graphics which could affect content, and all legal disclaimers and ethical guidelines that apply to the journal pertain. ACS cannot be held responsible for errors or consequences arising from the use of information contained in these “Just Accepted” manuscripts.

is published by the American Chemical Society. 1155 Sixteenth Street N.W., Washington, DC 20036 Published by American Chemical Society. Copyright © American Chemical Society. However, no copyright claim is made to original U.S. Government works, or works produced by employees of any Commonwealth realm Crown government in the course of their duties.

Page 1 of 29 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

ACS Applied Energy Materials

Sulfonated Terpolymers Containing Alkylene and Perfluoroalkylene Groups: Effect of Aliphatic Groups on Membrane Properties and Interface with the Catalyst Layers

Jinju Ahn† and Kenji Miyatake*,†,‡



Clean Energy Research Center and ‡Fuel Cell Nanomaterials Center, University of Yamanashi,

4-4-37 Takeda, Kofu, Yamanashi 400-8510, Japan Corresponding Author *E-mail: [email protected]. KEYWORDS: sulfonated terpolymers, perfluoroalkylene groups, proton conductive polymers, bendable thin membranes, fuel cells,

ACS Paragon Plus Environment

1

ACS Applied Energy Materials 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 2 of 29

ABSTRACT

Two series of terpolymers (SPA-A, -B and -C) composed of perfluoroalkylene, alkylene, and sulfonated phenylene (SP) groups were prepared to investigate the effect of aliphatic groups and their compositions onto the membrane properties for proton exchange membrane fuel cells. The composition of perfluoroalkylene (m) and alkylene groups (n) in SPA terpolymers was controlled to be m/n = 0.5/0.5 for SPA-A, 0.65/0.35 for SPA-B, and 1/0 for SPA-C. SPA terpolymers provided thin and bendable membranes with ion exchange capacity (IEC) ranging from 1.61 to 3.18 mequiv g-1. Introducing alkylene groups into the polymer main chain was effective in achieving high IEC values. SPA-B membranes with lower alkylene group content showed slightly more developed phase-separated morphology than that of SPA-A membranes with higher alkylene group content. The developed phase separation with interconnected ionic channels resulted in high proton conductivity for SPA-B membranes. The alkylene groups in the main chain also contributed to improving mechanical properties as suggested by stress versus strain curves, in which SPA membranes exhibited higher Young’s moduli and higher yield strength than those of copolymer (SPAF) membranes with no alkylene groups. An H2/O2 (or air) fuel cell with SPA-B membrane exhibited high open circuit voltage (OCV, 0.99 V at 100% RH with O2), low ohmic resistance (0.05 Ω cm2 at 100% RH with O2), and good current/voltage performance, reflecting the properties of SPA-B membrane. However, interfacial compatibility with the catalyst layers was somewhat deteriorated with SPA-B membrane to cause lower mass activity (70 A g-1 at 100% RH) of the cathode compared to that with SPAF membrane (102 A g-1 at 100% RH). SPA-B membrane was durable in OCV hold test for 1000 h with slight degradation in alkylene groups.

ACS Paragon Plus Environment

2

Page 3 of 29 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

ACS Applied Energy Materials

INTRODUCTION Polymer electrolyte membrane fuel cells (PEMFCs) have received considerable attention as an efficient and eco-friendly energy conversion device, in particular, for applications in electric vehicles and residential cogeneration systems.1 State-of-the-art and most used PEM materials are perfluorosulfonic acid (PFSA) polymer membranes (such as Nafion and Gore Select) because of their high proton conductivity, chemical and physical stability under fuel cell operating conditions. Although PFSA membranes have been contributing to commercialization and initial dissemination of PEMFCs, there is still a great demand for alternative PEM materials that overcome shortcomings of PFSAs; high production cost due to complicated manufacturing processes, narrow service temperature range below the glass transition temperature (ca. 110 ºC), and high gas permeability to reduce current efficiency and cause membrane degradation.2-5 In the literature, there have been a considerable number of reports on acid-functionalized polymeric materials for the purpose.6-9 Among them, sulfonated aromatic polymers and copolymers have been probably most investigated because of their large freedom in molecular design including main chain and side chain structures, sequences of copolymer components, positions and number of acidic groups, etc.10-15 Recently, we have successfully developed sulfonated polyphenylenes composed solely of sulfonic acid groups and phenylene rings.16 The polyphenylene ionomer membranes exhibited high proton conductivity and chemical stability leading to high fuel cell performance and durability. Unlike typical sulfonated aromatic (co)polymers, lack of heteroatom linkages such as ether, sulfide, and sulfone groups in the polyphenylene ionomer main chain was effective in achieving highly oxidative stability of the membranes. Similar results were obtained with other sulfonated polyphenylene membranes with more complicated structures.17

ACS Paragon Plus Environment

3

ACS Applied Energy Materials 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 4 of 29

In addition to the bulk properties, interfacial compatibility with the catalyst layers is highly crucial for PEMs in practically operating fuel cells. Since PFSA ionomers are generally used as proton conducting binders in the catalyst layers, incompatibility of the perfluorinated and nonfluorinated ionomer materials often impedes transport of protons and water at the interface of the catalyst layers and PEMs.18,19 In order to mitigate the interfacial issues, we have proposed partially fluorinated sulfonated polyphenylene (SPAF, Figure 1) membrane.20 Because of its well-defined molecular structure with small-scale phase-separated morphology similar to those of the PFSA membranes, SPAF membrane had an improved interfacial contact with the catalyst layers and exploited high cathode performance. The proton conductivity of SPAF membrane, however, still needed to be improved at low humidity condition.

F F SO3H

F F

F F

F F

F F

F F

m SO3H

n SO3H

o SO3H

Figure 1. Structure of partially fluorinated sulfonated polyphenylene (SPAF).

The objective of the present research is to synthesize a series of terpolymers (SPA) composed of sulfophenylene, perfluoroalkylene, and alkylene groups, and to evaluate the effect of the aliphatic components in the main chain onto the bulk and interfacial properties of the resulting PEMs. Three types of SPA membranes; SPA-A, -B and -C with different ion exchange capacities (IECs) were prepared by changing the terpolymer compositions. In the case of SPAF copolymers, high IEC and thus high proton conductivity could not be achieved partly because of the synthetic method via post-sulfonation.20 In the present study, introducing alkylene groups as the third

ACS Paragon Plus Environment

4

Page 5 of 29 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

ACS Applied Energy Materials

component and using pre-sulfonated monomer enabled us to obtain higher IEC terpolymer membranes. The properties of SPA membranes including proton conductivity, water absorbability, mechanical properties, and fuel cell performance and durability have been studied and compared with those of SPAF membrane.

RESULTS AND DISCUSSION Synthesis of Terpolymers (SPA).

A series of novel terpolymers (SPA) composed of

sulfonated phenylene, alkylene, and perfluoroalkylene groups was synthesized via Ni(0)promoted coupling reaction (Scheme 1). The feed ratio of the monomer 1 containing perfluoroalkylene group and the monomer 2 containing alkylene group was controlled so as to evaluate its effect on the membrane properties. The feed ratio of 2,5-dichlorobenzenesulfonic acid (SP) monomer to the aliphatic monomers (1 and 2) was adjusted to obtain SPA terpolymers with targeted IEC ranging from 1.7 to 3.4 mequiv g-1. The terpolymerization reaction proceeded well in DMSO solution to provide the corresponding products in high yields (~ 94%). The resulting terpolymers were soluble in polar organic solvents such as DMAc, DMSO, and NMP. The chemical structure of the terpolymers was analyzed by 1H and 19F NMR spectra (Figure 2). In the 1H NMR spectra, aromatic and aliphatic protons were assigned to the supposed structure although the composition of the components could not be determined due to the significant overlappings of the aromatic peaks. In the

19

F NMR spectra, three characteristic peaks for

perfluorohexylene groups were observed at slightly lower magnetic fields than those of the monomer 1. The results indicate successful formation of the targeted SPA terpolymers. The molecular weight of the SPA-A and -B terpolymers was estimated by GPC to be Mn = 61-104

ACS Paragon Plus Environment

5

ACS Applied Energy Materials 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 6 of 29

kDa and Mw = 134-183 kDa, respectively (Table 1 and Figure S1). SPA-C polymers were obtained in lower molecular weight, indicating lower reactivity of the monomer 1 than 2. The dispersity (PDI) was 1.7-2.2 and reasonable for this type of polycondensation reaction. The apparent molecular weight was higher with increasing the SP content presumably because of the larger radius of gyration of the terpolymers with higher IEC values (or higher content of the sulfonic acid groups).

Scheme 1. Synthesis of SPA terpolymers composed of perfluoroalkylene, alkylene, and sulfonated phenylene groups

ACS Paragon Plus Environment

6

Page 7 of 29 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

ACS Applied Energy Materials

Figure 2. (a) 1H and (b)19F NMR spectra of SPA terpolymer in DMSO-d6 at 80 ºC.

ACS Paragon Plus Environment

7

ACS Applied Energy Materials 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 8 of 29

Table 1. Physical Properties of SPA Membranes GPC (kDa)a Sample

A

B

IEC (mequiv g-1)

1(m) : 2 (n) : SP(o) Mn

Mw

Targetedb

Titratedc

0.50 : 0.50 : 1.04

61

134

1.7

1.61

0.50 : 0.50 : 2.14

77

153

2.8

2.55

0.50 : 0.50 : 3.17

93

161

3.4

3.18

0.65 : 0.35 : 1.04

64

139

1.7

1.58

0.65 : 0.35 : 2.14

88

168

2.8

2.51

0.65 : 0.35 : 3.17

104

183

3.4

3.11

1 : 0 : 1.10

13

64

1.7

1.52

1 : 0 : 1.85

5

34

2.5

-d

C

a

Determined by GPC (DMF containing 0.01 M LiBr was used as eluent). b Calculated from the feed monomer compositions assuming 100% conversion. c Obtained from titration. d Unavailable because a membrane was not obtained.

SPA-A and -B terpolymers provided thin, bendable, and brown membranes by casting from DMSO solution. SPA-B membranes were transparent while SPA-A membranes were slightly turbid reflecting the lower solubility of the latter terpolymers containing more alkylene groups. Similar behavior was observed in our previously reported ammonium containing copolymers.21 Because of its lower molecular weight, SPA-C with higher IEC (2.5 mequiv g-1) did not give a self-standing membrane. The IECs of the membranes were determined by acid-base titration. The resulting IEC values were only slightly lower (up to ca. 7%) than those calculated from the feed monomer ratios. It should be noted the high IEC values (> 2.0 mequiv g-1) were achievable

ACS Paragon Plus Environment

8

Page 9 of 29 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

ACS Applied Energy Materials

by introducing alkylene groups. The copolymerization of 1 and SP did not give high enough molecular weight copolymers to form self-standing membranes when the targeted IECs were higher than > 2.0 mequiv g-1 (results not shown).

Properties of SPA Membranes.

Figure 3 shows TEM images of SPA-A and SPA-B

membranes stained with Pb2+ ions. The black domains are related with hydrophilic domains containing stained sulfonic acid groups. SPA-B (IEC = 1.58 mequiv g-1) membrane with larger content of perfluoroalkylene groups than SPA-A (IEC = 1.61 mequiv g-1) membrane exhibited somewhat more distinct phase-separated morphology. In addition, the hydrophilic clusters were more interconnected for SPA-B than for SPA-A. The average sizes of the hydrophilic and hydrophobic clusters were 3.6 nm and 3.0 nm for SPA-A, and 5.3 nm and 3.0 nm for SPA-B, respectively. The hydrophilic/hydrophobic difference of the components was more pronounced in SPA-B than in SPA-A, which must be responsible for such morphological differences. In the TEM images of SPA-B with higher IECs (2.51 and 3.11 mequiv g-1), larger hydrophilic clusters (~ ca. 8 nm) were observed presumably because of the larger content of the ionic groups. Compared

to

the

SPAF

membrane

with

lower

IEC

(1.59

mequiv

g-1),20

the

hydrophilic/hydrophobic domain sizes were similar but their interfaces were less distinct probably because of less hydrophobicity of the alkylene groups as the third component than the perfluoroalkylene groups.

ACS Paragon Plus Environment

9

ACS Applied Energy Materials 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 10 of 29

Monomer 1(m) : Monomer 2(n) : SP (o)

Figure 3. TEM images of SPA membranes stained with Pb2+ ions; (a) SPA-A membrane (IEC 1.61 mequiv g-1), (b) SPA-B membrane (IEC 1.58 mequiv g-1), (c) SPA-B membrane (IEC 2.51 mequiv g-1) and (d) SPA-B membrane (IEC 3.11 mequiv g-1), respectively. The ratios in the images represent the feed monomer ratios.

ACS Paragon Plus Environment

10

60 50 (a) 40 30 20 10 0 100 (b)

Proton conductivity / S cm -1

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

ACS Applied Energy Materials

Water uptake, %

Page 11 of 29

10-1 10-2 SPA-A IEC1.61 IEC2.55 IEC3.18 SPA-B IEC1.58 IEC2.51 IEC3.11 SPA-C IEC1.52 NRE212

10-3 10-4 10-5 0

20

40

60

80

100

Relative humidity, % Figure 4. Humidity dependence of (a) water uptake and (b) proton conductivity of SPA and Nafion NRE212 membranes at 80 ºC.

ACS Paragon Plus Environment

11

ACS Applied Energy Materials 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 12 of 29

Figure S2 shows SAXS profiles of SPA-B membranes measured at 30-90% relative humidity (RH) and 80 ºC. While high IEC SPA-B (IEC = 3.0 mequiv g-1) membrane did not show peaks, lower IEC SPA-B (IEC = 1.5 and 2.5 mequiv g-1) membranes exhibited a peak at ca. d = 20 nm. The peak became smaller as increasing the humidity suggesting that it is associated with the hydrophobic domains (or matrix knee). At 90% RH, another broad peak appeared at ca. d = 8 nm for the three membranes, presumably attributable to periodic structure of ionic domains. Compared to SPAF (IEC = 1.59 mequiv g-1) membrane,20 the d values at higher scattering vector (q) were larger for SPA membranes. Figure 4 shows proton conductivity and water uptake of SPA membranes at 80 ºC as a function of relative humidity (RH). For reference, data for Nafion NRE212 membrane is also included. Water uptake and proton conductivity increased with increasing IEC for the SPA membranes. The water uptake of SPA-A and SPA-B membranes with similar IECs was comparable at a wide range of humidity, indicating minor effect of the composition of the hydrophobic components on the water affinity of the membranes. In other words, the sulfonic acid groups were hydrated to the similar levels in both series of the membranes. Despite their similar water affinity, SPA-B membranes exhibited slightly higher proton conductivities than those of SPA-A membranes. As discussed with the TEM images above, SPA-B contained more interconnected ionic channels which should be responsible for higher proton conductivity. SPA-C membrane (1.52 mequiv g-1) without alkylene groups in the main chain exhibited higher proton conductivity than those of SPA-A and -B membranes, in particular, at low humidity. The high IEC SPA-A (3.18 mequiv g1

) and -B (3.11 mequiv g-1) membranes exhibited comparable or higher proton conductivity

compared to Nafion NRE 212 membrane at a wide range of humidity. These membranes outperformed SPA-C (1.59 mequiv g-1) membrane because of the higher IEC values. The proton

ACS Paragon Plus Environment

12

Page 13 of 29 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

ACS Applied Energy Materials

conductivities of SPA-A, SPA-B, and SPA-C membranes were 2.3, 1.8, 3.2 mS cm-1 at 30% RH, respectively. Temperature dependence of water uptake and proton conductivity of SPA-B (IEC 2.51 mequiv. g-1) membrane was measured (Figure S3). The membrane retained its high conductivity up to 120 ºC while lost water uptake slightly. Humidity dependence of the storage modulus (E’), the loss modulus (E’’), and tan δ (= E’’/E’) of the SPA membranes was investigated by dynamic mechanical analysis (DMA) at 80 ºC as shown in Figure 5. SPA-A and SPA-B membranes exhibited similar viscoelastic properties without obvious transition behavior under the given conditions. The storage modulus decreased with increasing humidity for both series of the membranes, suggesting that absorbed water molecules soften the membranes. SPA-C membrane showed larger loss in E’ and E’’ at high humidity compared to those of SPA-A and -B membranes due to its lower molecular weight.

ACS Paragon Plus Environment

13

ACS Applied Energy Materials

1010 (a)

(d)

(g)

SPA-A IEC 1.61 IEC 2.55 IEC 3.18

SPA-B IEC 1.58 IEC 2.51 IEC 3.11

SPA-C IEC 1.52

(b)

(e)

(h)

(c)

(f)

(i)

E' / Pa

9

10

108 7

10

E'' / Pa

109 8

10

107 106 100

tan δ

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 14 of 29

10-1

10-2 0

20 40 60 80 Relative humidity, %

0

20 40 60 80 Relative humidity, %

0

20 40 60 Relative humidity, %

80

Figure 5. Dynamic mechanical analyses of SPA membranes at 80 ºC as a function of the relative humidity: (a) E’, (b) E’’ and (c) tan σ of SPA-A, (d) E’, (e) E’’ and (f) tan σ of SPA-B, and (g) E’, (h) E’’ and (i) tan σ of SPA-C, respectively.

ACS Paragon Plus Environment

14

Page 15 of 29

Figure 6 shows tensile test results (stress/strain curves) of SPA membranes at 80 ºC and 60% RH. SPA-A and SPA-B membranes exhibited similar elongation properties with the Young’s moduli (0.9 - 2.5 GPa and 0.5 - 2.5 GPa), yield strengths (7.6 - 15 MPa and 4.9 - 12 MPa), and tenstile strains (15 - 81% and 12 - 99%), respectively, depending on their IEC. Briefly, as increasing the IEC value, the maximum strain decreased and the Young’s modulus and yield strength increased (Table 2). Compared to SPA-C membrane (1.52 mequiv g-1), SPA-A and -B membranes with similar IEC (1.61 and 1.58 mequiv g-1, respectively) exhibited higher Young’s moduli, higher yield strengths, and comparable maximum strains, similar to the DMA data mentioned above.

16 SPA-A SPA-B SPA-C IEC 1.61 IEC 1.58 IEC 1.52 IEC 2.55 IEC 2.51 IEC 3.18 IEC 3.11

12

Stress / MPa

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

ACS Applied Energy Materials

8

4

0 0

20

40

60

80

100

Strain, %

Figure 6. Stress versus strain curves of SPA membranes at 80 ºC and 60% RH.

ACS Paragon Plus Environment

15

ACS Applied Energy Materials 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 16 of 29

Table 2. Summary of Tensile Test Results of SPA-A, -B, and -C Membranes.

Membrane

SPA-A

SPA-B

SPA-C

IEC

Maximum

Young's modulus

Yield strength

(mequiv g )

strain (%)

(GPa)

(MPa)

1.61

80.6

0.9

7.6

2.55

26.6

2.7

14.6

3.18

14.5

2.5

15.0

1.58

98.7

0.5

4.9

2.51

25.7

2.2

11.1

3.11

11.5

2.5

12.0

1.52

89.0

0.3

3.7

-1

Fuel Cell Performance and Durability of SPA Membrane.

Because of the balanced

properties of water uptake, proton conductivity, mechanical properties, and their humidity dependence, SPA-B (IEC 2.51 mequiv g-1) was chosen for fuel cell evaluation. A membrane electrode assembly (MEA) was prepared from the SPA-B membrane (29 µm thick) with catalyst layers consisting of Pt/CB catalyst and Nafion binder for both the anode and the cathode. To evaluate the hydrogen permeability of the membrane, linear sweep voltammograms (LSVs) were measured at 80 ºC supplying humidified hydrogen and nitrogen to the anode and cathode, respectively, (Figure 7) prior to the performance evaluation. The oxidation current density of the permeated hydrogen was very small (ca. 3 µA cm-2) at 30% RH and higher (0.42-0.50 mA cm-2) at 100% RH. The hydrogen permeability of the SPA-B membrane was comparable to that of the

ACS Paragon Plus Environment

16

Page 17 of 29

SPAF membrane (0.40 mA cm-2 at 100% RH, 28 µm thick)20 and much smaller than that of Nafion NRE 212 membrane (1.45 mA cm-2 at 100% RH, 50 µm thick).

Current density / mA cm-2

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

ACS Applied Energy Materials

0.2 80 oC

30% RH 100% RH

0.1

0

-0.1 0.1

0.2

0.3 0.4 0.5 0.6 Potential vs. RHE / V

0.7

Figure 7. Linear sweep voltammograms (LSVs) of fuel cell with SPA-B (IEC = 2.51 mequiv g-) membrane at 80 ºC, 30% RH and 100% RH.

Figure 8 shows polarization curves (ohmic (IR) drop-included) and ohmic resistances of the fuel cell with the SPA-B membrane operated with hydrogen and oxygen or air at 80 ºC, 100% RH and 30% RH. The open circuit voltages (OCVs) were 0.99 V (oxygen, 100% RH), 0.96 V (air, 100% RH), 1.01 V (oxygen, 30% RH), and 0.97 V (air, 30% RH), respectively. The high OCV values support low hydrogen permeability of the membrane as suggested by LSVs. At 100% RH, the ohmic resistance was 0.05 Ω cm2 both with oxygen and air, which was only slightly higher than that (0.02 Ω cm2) calculated from the proton conductivity (Figure 4b) and the thickness of the membrane. The results indicate reasonably good interfacial contact between the SPA-B membrane and the Nafion-based catalyst layer. At 30% RH, the ohmic resistance was ca. 0.4 Ω

ACS Paragon Plus Environment

17

ACS Applied Energy Materials

cm2 at OCV and decreased with increasing the current density to 0.11 Ω cm2 with oxygen and 0.26 Ω cm2 with air, which were lower than that (0.51 Ω cm2) calculated from the proton conductivity and the thickness. The lower ohmic resistances in the operating fuel cell resulted from the back-diffusion of water from the cathode to the membrane. The effect was more pronounced with oxygen than with air since the oxygen flow rate (0.038 mL min-1 at 1 A cm-2) was slower than air flow rate (0.182 mL min-1 at 1 A cm-2) to have the same oxygen utility (40%). The ohmic resistance of SPA-B cell at 30% RH was smaller than that (0.33 Ω cm2 with air) of SPAF (IEC = 1.59 mequiv g-1)-cell due to the former’s higher IEC and higher proton conductivity. Compared to Nafion NRE212 membrane, the fuel cell performance of SPA-B

1.0 (a) 100%RH

AIR 1.0 O2

0.8

0.8

0.6

0.6

0.4

0.4

0.2

0.2 0

1.0 (b) 30%RH

1.0

0.8

0.8

0.6

0.6

0.4

0.4

0.2

0.2

0

0

0.5 1.0 -2 Current density / A cm

1.5

Ohmic resistance/ Ω cm2

0

Ohmic resistance/ Ω cm2

membrane was slightly lower under the same conditions (Figure S4).

Cell voltage(IR included) / V Cell voltage(IR included) / V

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 18 of 29

0

ACS Paragon Plus Environment

18

Page 19 of 29 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

ACS Applied Energy Materials

Figure 8. IR-included polarization curves and ohmic resistances of fuel cell with SPA-B membrane (IEC = 2.51 mequiv g-1) at 80 ºC under humidity conditions (a) 100% and (b) 30% RH.

In order to evaluate the compatibility of the SPA-B membrane and the Nafion-based catalyst layer in more details, IR-corrected IV curves were plotted (Figure S5) and mass activities (MAs) of the Pt catalysts in the cathode at 0.85 V were calculated therefrom. The MAs of the SPA-B cell with air were 70 A g-1 at 100% RH and 48 A g-1 at 30% RH, respectively, which were lower than those of the SPAF cell (102A g-1 at 100% RH and 51 A g-1 at 30% RH) under the same operating conditions (please note, however, that the used cells were different between SPA-B (original cell with 4.4 cm2 of the electrode area) and SPAF (JARI standard cell with 36 cm2 of the electrode area) membranes).20 Despite its higher proton conductivity and similarly phaseseparated morphology, SPA-B cell exhibited lower mass transport capability at the interface of the membrane/cathode

catalyst

layer than

that

of the SPAF cell.

Less

distinct

hydrophobic/hydrophilic phase separations would be responsible, in particular, at low humidity where proton transport to the catalyst surface became more crucial. In addition, higher IEC SPAB membrane showed higher water uptake than that of SPAF membrane, which might have caused local interfacial disconnection between SPA-B membrane and the Nafion-based catalyst layers (local delamination of the membrane from the catalyst layers). To evaluate the durability of the SPA-B membrane, OCV hold test was carried out with hydrogen and air (Figure 9). The OCV was initially 0.98 V and decreased to 0.86 V after 1000 h with the average decay of -120 µV/h. No sudden drop of OCV was observed during the test,

ACS Paragon Plus Environment

19

ACS Applied Energy Materials 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 20 of 29

indicating no serious damages on the membrane such as pinholes. After the OCV hold test for 1000 h, the IV performance was re-evaluated under the same operating conditions as above (Figure 10). The OCV decreased after the test from 0.99 V to 0.95 V (oxygen, 100% RH), 0.96 V to 0.91 V (air, 100% RH), 1.01 V to 0.85 V (oxygen, 30% RH), and 0.97 V to 0.90V (air, 30% RH), respectively. Durability of OCV in the SPA-B cell was better than that in SPAF membrane.20 The post-OCV hold test cell exhibited lower fuel cell performances than those of the pristine membrane cell. The loss in the performances, however, was not significant but rather minor with oxygen at 100% RH, followed by air at 100% RH and oxygen at 30% RH, and air at 30% RH. Since the ohmic resistances of the post-OCV hold test cell were similar to those of the pristine membrane (except for air at 30% RH), the lowered fuel cell performances were more likely caused by the degradation of the Nafion-based catalyst layers. This idea was supported by the IR-corrected curves in Figure S6, where the lower cathode performances were confirmed with the post-OCV hold test cell. The results support minor degradation of the SPA-B membrane under the test conditions. The local delamination of the membrane that might have further proceeded during the OCV hold test would be accountable for lower cathode performance.

ACS Paragon Plus Environment

20

Page 21 of 29

1.0 Cell voltage / V

0.9 0.8 0.7 0.6 0.5 0.4

0

200

400 600 Time / h

800

1000

Figure 9. OCV hold test of SPA-B cell (IEC = 2.51 mequiv g-1) at 80 ºC and 30% RH.

Ohmic resistance/ Ω cm2 Cell voltage(IR included) / V

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

ACS Applied Energy Materials

Air 100%RH 30%RH Before After

(a)

1.0

O2 100%RH 30%RH Before After

(c)

0.8 0.6 0.4 0.2 0.6 0.5 (b)

(d)

0.4 0.3 0.2 0.1 0

0

0.5 1.0 Current density / A cm -2

1.5

0

0.5 1.0 Current density / A cm -2

1.5

Figure 10. IR-included polarization curves and ohmic resistances of the fuel cell of SPA-B membrane before and after the OCV hold test: (a) and (b) with air, and (c) and (d) with oxygen at 80 °C, 100% and 30%RH.

ACS Paragon Plus Environment

21

ACS Applied Energy Materials

The fuel cell was disassembled and the SPA-B membrane was recovered by carefully removing the catalyst layers from both sides of the membrane to analyze the changes in the molecular weight and chemical structure. The recovered SPA-B membrane was still bandable. The GPC curves of the post-test SPA-B shifted to the longer retention time resulting in the lower numberaveraged molecular weight (Mn = 30 kDa) with larger dispersity (PDI = 7.0) than those of the pristine SPA membrane (Figure 11).

19

F NMR spectrum did not show practical changes

suggesting chemical robustness of the perfluoroalkylene groups (Figure 12a). In contrast, the 1H NMR spectrum of the post-test SPA-B membrane differed from that of the pristine membrane (Figure 12b). The peaks assignable to the aliphatic protons (no. 9-11) and aromatic protons (no. 5-8 and 12-14) were smaller for the post-test membrane. The results suggest some degradation of the components derived from the monomer 2, accountable for slightly higher ohmic resistance of the post-test fuel cell with air at 30% RH.

UV absorbance at 270 nm / a.u.

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 22 of 29

OCV test Before After

5

10 retention time / min

15

Figure 11. GPC profiles of SPA-B membrane before and after the OCV hold test.

ACS Paragon Plus Environment

22

Page 23 of 29 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

ACS Applied Energy Materials

Figure 12. (a) 19F and (b) 1H NMR spectra of SPA-B membrane before and after the OCV hold test in DMSO-d6 at 80 oC.

ACS Paragon Plus Environment

23

ACS Applied Energy Materials 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 24 of 29

CONCLUSIONS We have successfully synthesized two types of sulfonated terpolymers (SPA) containing perfluoroalkylene and alkylene groups to investigate the effect of these (perfluorinated) aliphatic groups on the membrane and interface properties. Both series of terpolymers provided bendable membranes by solution casting. Introducing alkylene groups enabled higher IEC membranes than the previous sulfonated copolymer (SPAF) membranes without alkylene groups. Effect of the aliphatic groups on the membrane properties was significant. Because of the less hydrophobic nature of the alkylene groups than the perfluoroalkylene groups, the hydrophilic/hydrophobic phase-separated morphology of SPA-A membranes with higher alkylene content was less distinct. SPA-B membranes exhibited slightly higher proton conductivity and similar water uptake compared to those of SPA-A membranes reflecting more developed morphology of the formers ones with better interconnected ionic channels. Because of IEC higher than that of SPAF membrane, SPA membranes showed much higher proton conductivity. The alkylene groups in the main chain also impacted on the mechanical properties. SPA-A and -B membranes exhibited higher Young’s moduli, higher yield strengths and comparable maximum strains compared to those of SPA-C membrane. The SPA-B membrane showed very low hydrogen permeability as suggested by low hydrogen oxidation current densities in LSVs and high OCVs in a fuel cell. The ohmic resistance of the fuel cell was reasonable for high proton conductivity of the SPA-B membrane. The compatibility of the SPAB membrane with Nafion-based catalyst layers was not as good as that of SPAF membrane probably because of the inefficient mass transport capability at their interfaces in particular at low humidity. The OCV hold test of the fuel cell revealed high oxidative durability of the SAP-B membrane with small loss in OCV value (the average decay of -120 µV/h) for 1000 h. The post

ACS Paragon Plus Environment

24

Page 25 of 29 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

ACS Applied Energy Materials

durability analyses of the SPA-B membrane suggested small but not severe degradation in the alkylene groups in the main chain. By tuning the alkylene chain length and/or terpolymer composition, imcompatibility with the catalyst layers and chemical vulnerability would be mitigated.

ASSOCIATED CONTENT Supporting Information The Supporting Information is available free of charge on the ACS Publications website at DOI: . Experimental details and additional experimental data (PDF) AUTHOR INFORMATION Corresponding Author *E-mail: [email protected]. Notes The authors declare no competing financial interest. ACKNOWLEDGMENTS This work was partly supported by the New Energy and Industrial Technology Development Organization (NEDO) through the SPer-FC Project and the Ministry of Education, Culture, Sports, Science and Technology (MEXT) Japan through a Grant-in-Aid for Scientific Research (18H02030).

ACS Paragon Plus Environment

25

ACS Applied Energy Materials 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 26 of 29

REFERENCES (1) Carrette, L.; Friedrich, KA.; Stimming, U. Fuel Cells: Principles, Types, Fuels, and Applications. Fuel Cells 2001, 1, 5-39. (2) Mauritz, K. A.; Moore, R. B.; State of Understanding of Nafion. Chem. Rev. 2004, 104, 4535-4586. (3) Curtin, D. E.; Lousenberg, R. D.; Henry, T. J.; Tangeman, P. C.; Tisack, M. E. Advanced Materials for Improved PEMFC Performance and Life. J. Power Sources 2004, 131, 41-48. (4) Broka, K.; Ekdunge, P. Oxygen and Hydrogen Permeation Properties and Water Uptake of Nafion 117 Membrane and Recast Film for PEM Fuel Cell. J. Appl. Electrochem. 1997, 27, 117-123. (5) Tang, Y.; Karlsson, A. M.; Santare, M. H.; Gilbert, M.; Johnson, W. B. An Experimental Investigation of Humidity and Temperature Effects on the Mechanical Properties of Perfluorosulfonic acid Membrane. Mater. Sci. Eng. 2006, 425, 297-304. (6) Hickner, M. A.; Ghassemi, H.; Kim, Y. S.; Einsla, B. R.; McGrath, J. E. Alternative Polymer Systems for Proton Exchange Membranes. Chem. Rev. 2004, 104, 4587-4612. (7) Zhang, H., Shen, P. K., Recent Development of Polymer Electrolyte Membranes for Fuel Cell. Chem. Rev. 2012, 112, 2780-2832. (8) Higashihara, T.; Matsumoto, K.; Ueda, M. Sulfonated Aromatic Hydrocarbon Polymers as Proton Exchange Membranes for Fuel Cells. Polymer 2009, 50, 5341-5357. (9) Miyake, J.; Miyatake, K. Fluorine-free Sulfonated Aromatic Polymers as Proton Exchange Membranes. Polym. J, 2017, 49, 487-495.

ACS Paragon Plus Environment

26

Page 27 of 29 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

ACS Applied Energy Materials

(10) Park, C. H.; Lee, C. H.; Guiver, M. D.; Lee, Y. M. Sulfonated Hydrocarbon Membranes for Medium-Temperature and Low-Humidity Proton Exchange Membrane Fuel Cells (PEMFCs), Prog. Polym. Sci. 2011, 36, 1443-1498. (11) Peckham, T. J.; Schmeisser, J.; Rodgers, M.; Holdcroft, S. Main-chain, Statistically Sulfonated Proton Exchange Membranes: the Relationships of Acid Concentration and Proton Mobility to Water Content and their Effect upon Proton Conductivity. J. Mater. Chem. 2007, 17, 3255. (12) Ahn, J.; Lee, H.; Yang, T.; Kim, C.; Bae, B. Synthesis and Characterization of Multi-Block Sulfonated Poly(arylene ether sulfone) Membranes with Different Hydrophilic Moieties for Application in Polymer Electrolyte Membrane Fuel Cell. J. Polym. Sci., A: Polym. Chem. 2014, 52, 2947-2957 (13) Xie, H.; Tao, D.; Xiang, X.; Ou, Y.; Bai, X.; Wang, L. Synthesis and Properties of Highly Branched Star-Shaped Sulfonated Block Poly(arylene ether)s as Proton Exchange Membranes. J. Membr. Sci. 2015, 473, 226-236. (14) Moh, L. C. H, Goods, J. B., Kim, Y.; Swager, T. M. Free Volume Enhanced Proton Exchange Membranes from Sulfonated Triptycene Poly(ether ketone). J. Membr. Sci. 2018, 549, 236-243. (15) Miyake, J.; Mochizuki, T.; Miyatake, K. Effect of the Hydrophilic Component in Aromatic Ionomers: Simple Structure Provides Improved Properties as Fuel Cell Membranes. ACS Macro Lett. 2015, 4, 750-754. (16) Miyake, J.; Taki, R.; Mochizuki, T.; Shimizu, T.; Akiyama, R.; Uchida, M.; Miyatake, K. Design of Flexible Polyphenylene Proton-Conducting Membrane for Next-Generation Fuel Cells. Sci. Adv. 2017, 3, eaao0476.

ACS Paragon Plus Environment

27

ACS Applied Energy Materials 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 28 of 29

(17) Adamski, M.; Skalski, T, J, G.; Britton, B.; Peckham, T. J.; Metzler, L.; Holdcroft, S. Highly Stable, Low Gas Crossover, Proton-Conducting Phenylated Polyphenylenes. Angew. Chem. 2017, 129, 9186-9189. (18) Oh, K.; Kang, H. S.; Choo, M.; Jang, D.; Lee, D.; Lee, D. G.; Kim, T.; Hong, Y. T.; Park, J.; Kim, H. Interlocking Membrane/Catalyst Layer Interface for High Mechanical Robustness of Hydrocarbon-Membrane-Based Polymer Electrolyte Membrane Fuel Cells. Adv. Mater. 2015, 27, 2974-2980. (19) Afsahi, F.; Mathieu-Potvin, F.; Kaliaguine, S. Impact of Ionomer Content on Proton Exchange Membrane Fuel Cell Performance. Fuel Cells 2016, 1, 107-125. (20) Mochizuki, T.; Uchida, M.; Miyatake, K. Simple, Effective Molecular Strategy for the Design of Fuel Cell Membranes: Combination of Perfluoroalkyl and Sulfonated Phenylene Groups. ACS Energy Lett. 2016, 1, 348-352. (21) Ono, H.; Miyake, J.; Miyatake, K. Partially Fluorinated and Ammonium-Functionalized Terpolymers: Effect of Aliphatic Groups on the Properties of Anion Conductive Membranes. J. Polym. Sci., A: Polym. Chem. 2017, 55, 1442-1450. (22) Mochizuki, T.; Uchida, M.; Uchida, H.; Watanabe, M.; Miyatake, K.; Double-layer Ionomer Membrane for Improving Fuel Cell, ACS Appl. Mater. Interfaces, 2014, 6, 1389413899

ACS Paragon Plus Environment

28

Page 29 of 29 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

ACS Applied Energy Materials

TOC GRAPHIC

ACS Paragon Plus Environment

29