Surface Modification of Pollen-Shape Carriers for Dry Powder

Dec 4, 2014 - Surface modification of pollen-shape hydroxyapatite (HA) carriers is achieved using surface etching technique. Characterization of HA ca...
2 downloads 0 Views 2MB Size
Subscriber access provided by UNIV NEW ORLEANS

Article

Surface modification of pollen-shape carriers for dry powder inhalation through surface etching Thi Quynh Ngoc Nguyen, Hung Loong Giam, Yabo Wang, Adam Pac#awski, Jakub Szl#k, Aleksander Mendyk, Yu-Hsuan Shao, and Raymond Lau Ind. Eng. Chem. Res., Just Accepted Manuscript • DOI: 10.1021/ie502980k • Publication Date (Web): 04 Dec 2014 Downloaded from http://pubs.acs.org on December 10, 2014

Just Accepted “Just Accepted” manuscripts have been peer-reviewed and accepted for publication. They are posted online prior to technical editing, formatting for publication and author proofing. The American Chemical Society provides “Just Accepted” as a free service to the research community to expedite the dissemination of scientific material as soon as possible after acceptance. “Just Accepted” manuscripts appear in full in PDF format accompanied by an HTML abstract. “Just Accepted” manuscripts have been fully peer reviewed, but should not be considered the official version of record. They are accessible to all readers and citable by the Digital Object Identifier (DOI®). “Just Accepted” is an optional service offered to authors. Therefore, the “Just Accepted” Web site may not include all articles that will be published in the journal. After a manuscript is technically edited and formatted, it will be removed from the “Just Accepted” Web site and published as an ASAP article. Note that technical editing may introduce minor changes to the manuscript text and/or graphics which could affect content, and all legal disclaimers and ethical guidelines that apply to the journal pertain. ACS cannot be held responsible for errors or consequences arising from the use of information contained in these “Just Accepted” manuscripts.

Industrial & Engineering Chemistry Research is published by the American Chemical Society. 1155 Sixteenth Street N.W., Washington, DC 20036 Published by American Chemical Society. Copyright © American Chemical Society. However, no copyright claim is made to original U.S. Government works, or works produced by employees of any Commonwealth realm Crown government in the course of their duties.

Page 1 of 28

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Industrial & Engineering Chemistry Research

1

Surface modification of pollen-shape carriers for dry powder inhalation through surface

2

etching

3 4

Thi Quynh Ngoc Nguyen,† Hung Loong Giam,† Yabo Wang,† Adam Pacławski,‡ Jakub Szlęk,‡

5

Aleksander Mendyk,‡ Yu-Hsuan Shao,*,§ and Raymond Lau*,†

6 7



8

Nanyang Drive, Singapore 637459

9



School of Chemical and Biomedical Engineering, Nanyang Technological University, 62

Department of Pharmaceutical Technology and Biopharmaceutics, Jagiellonian University

10

Medical College, Medyczna 9 St, 30-688 Krakow, Poland

11

§

12

Taipei City, Taiwan 110

13

Abstract

Graduate Institute of Biomedical Informatics, Taipei Medical University, 250 Wu-Hsing Street,

14

Surface modification of pollen-shape hydroxyapatite (HA) carriers is achieved using

15

surface etching technique. Characterization of HA carriers before and after etching are

16

performed by scanning electron microscopy (SEM), Carr’s compressibility index (CI), X-ray

17

diffraction (XRD), and thermogravimetric analysis (TGA). Four surface etching temperatures are

18

tested but only the particles etched at 40ºC and 50ºC are found satisfactory. Proper surface

19

etching allows a reduction of the petal-like structure on the particle surface and improves the

20

crystallinity of the particles. While the reduction of petal-like structure decreases the emitted

21

dose (ED) of the drug particles, an increase in fine particle fraction (FPF) can be attained owing

22

to the improvement in drug liberation. An increase in the air flow rate, however decreases the *

Corresponding author. Tel.: +65 6316 8830 (R. Lau); +886 2-2736-1661-3356 (Y.-H. Shao) Email addresses: [email protected] (R. Lau); [email protected] (Y.-H. Shao)

1

ACS Paragon Plus Environment

Industrial & Engineering Chemistry Research

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

23

significance of particle surface morphology and the difference in FPF among the used of

24

different carrier particles diminishes. Surface etching technique is found to have good potential

25

as an economical process to improve dry powder inhalation efficiency through surface

26

modification.

27 28

Keywords: dry powder inhalation, drug carrier, surface etching, in vitro deposition, emitted

29

dose, fine particle fraction

30

2

ACS Paragon Plus Environment

Page 2 of 28

Page 3 of 28

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

31

Industrial & Engineering Chemistry Research

Introduction

32

The use of pollen-shape drug carriers in dry powder inhalation (DPI) has been found to

33

have a great potential in the delivery of powdered drugs through inhalation1-6. The pollen-shape

34

carriers are capable of achieving a higher emitted dose (ED) and fine particle fraction (FPF)

35

compared to irregular-shape lactose carriers1,2. The pollen-shape surface allows a long time of

36

flight for the detachment of drug to take place. In addition, pollen-shaped carriers have large

37

surface areas and binding sites that allow high drug attachment capacity. Both factors contribute

38

to the high ED and FPF achieved1,2. Based on the regional deposition results, it is found that the

39

high drug attachment characteristics of the pollen-shape carriers also restrict the drug liberation

40

during inhalation. It is anticipated that the FPF can be further improved by reducing the surface

41

interaction between the carriers and the drugs. However, reduction of particle adhesion can also

42

lower the ED4,7-9. It is important to strive for a balance between the attachment and the liberation

43

of drugs at the carrier surfaces.

44

Several approaches have been proposed to reduce the interaction between particles, such as

45

the use of spacer particles10, addition of nano/micro-particles11-13, surface coating14,15, etc. While

46

these approaches have shown satisfactory results in a number of studies, the effect is specific to

47

the carrier particles applied. The use of spacer particles and nanoparticles was found to give

48

negligible improvement on the performance pollen-shape carriers. It is also a great challenge to

49

apply surface coating on the pollen-shape surfaces. Thus, surface etching is proposed in this

50

study as an alternative surface modification method to reduce the surface interactions.

51

The surface etching technique involves the dissolution of the carrier surface partially in an

52

etching solution. The etching solution can be an acid or a saturated solution of the same or

53

similar composition as the carrier particles. Acid has the ability to dissolve many types of

3

ACS Paragon Plus Environment

Industrial & Engineering Chemistry Research

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

54

organic or inorganic compounds. The degree of dissolution is dependent on the dissolution time

55

and the concentration of the acid16. It has been reported in the literature that the dissolution

56

mechanism of hydroxyapatite starts with the formation of dissolution nuclei17. The nuclei appear

57

most likely on inhomogeneous surfaces and both polynuclear dissolution and etch pits formation

58

mechanisms can happen simultaneously17,18. Alternatively, the carrier particles can be mixed

59

with a saturated solution of the same composition19. A subsequent increase in temperature can

60

increase the solubility of the solution. Certain parts of the carrier surface can be dissolved and

61

hence achieved surface etching. The use of surface etching causes minimal change in the

62

material properties of the original particles. The simple nature of the process allows a good

63

potential in scale-up and utilization in the pharmaceutical industry.

64

In this study, the modification of pollen-shape carrier surfaces by surface etching through

65

temperature control is explored. Pollen-shape hydroxyapatite (HA) particles are used the carriers.

66

HA has the chemical formula of Ca5(PO4)3(OH). Saturated solution of phosphate salt is used as

67

the etching solution. The HA particles before and after surface etching are characterized by

68

scanning electron microscopy (SEM), Carr’s compressibility index (CI), X-ray diffraction

69

(XRD), and thermogravimetric analysis (TGA). The in vitro aerosolization and deposition

70

properties of the modified and original HA carriers are also determined using Budesonide (Bd)

71

as the model drug using Andersen cascade impactor (ACI).

72 73

Experimental

74

Preparation of HA

75

Hydroxyapatite (HA, Ca5(PO4)3(OH)) particles are synthesized by hydrothermal reaction

76

of potassium dihydrogen phosphate (KH2PO4, Sigma-Aldrich) and calcium nitrate tetrahydrate

4

ACS Paragon Plus Environment

Page 4 of 28

Page 5 of 28

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Industrial & Engineering Chemistry Research

77

(Ca(NO3)2.4H2O, Sigma-Aldrich). The resulting pollen-shape morphology is governed by the

78

synthesis temperature and the concentrations of poly (sodium-4-styrene sulfonate) (PSS, Sigma-

79

Aldrich) and urea (Sigma-Aldrich) used. The synthesis condition used in this study is following

80

the one used in a previous study2. 60 mL of KH2PO4 (0.02 M) solution is mixed with 100 mL of

81

Ca(NO3)2.4H2O (0.02 M) solution. Subsequently, sufficient PSS and urea are added to obtain a

82

respective concentration of 40 g/L and 0.5 M. The final mixture is stirred for 30 minutes to allow

83

complete dissolution of the urea. The solution mixture is then kept in an autoclave and put into

84

an oven. A reaction temperature of 120ºC is maintained for 6 hours. The final precipitated

85

product is then filtered, washed, and dried at 80ºC.

86 87

Surface Etching

88

A saturated solution of potassium dihydrogen phosphate, KH2PO4 is used as the etching

89

solution. 20 g of KH2PO4 is mixed with 100 mL of distilled water. The amount of KH2PO4 added

90

exceeds the solubility limit of KH2PO4 in distilled water. Upon constant stirring of 30 minutes,

91

the undissolved KH2PO4 is filtered. Afterwards, HA carriers are introduced to the saturated

92

KH2PO4 solution. A constant stirring is maintained to suspend the carriers in the solution. The

93

suspension temperature is then raised to a desired point slowly by a heater. The carriers are

94

allowed to re-dissolve into the solution at the desired temperature for 15–30 minutes and hence

95

the carrier surface is etched. The resulting HA carriers are finally filtered, washed, and dried at

96

80ºC. Four surface etching temperatures, 30ºC, 40ºC, 50ºC, and 60ºC are being explored in this

97

study.

98

5

ACS Paragon Plus Environment

Industrial & Engineering Chemistry Research

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

99

Page 6 of 28

Shape and Surface Morphology

100

The physical properties such as the shape and surface morphology of the HA carriers are

101

characterized by the scanning electron microscope (SEM) (JSM-5600, JEOL, Tokyo, Japan).

102

Dry HA particles are placed uniformly on a carbon tape attached on a stub. The particles are then

103

coated with platinum under an argon atmosphere (JFC-1600, JEOL, Auto Fine Coater, Tokyo,

104

Japan) for 60 seconds with a current of 20 mA. SEM images are taken at random locations over

105

the coated particles to obtain an overall indication of the particle physical properties.

106 107

Particle Densities and Flowability

108

The bulk density (ρbulk) and tap density (ρtap) of the particles can be used to give an

109

indication of the particle flowability. 100 mg of a sample is placed in a 1 mL micro-syringe. The

110

syringe tube is then tapped against a tabletop by hand at a rate of about 4 times per second for

111

2,000–2,500 times until no reduction in the sample volume is noticed. The volumes of the

112

sample before and after tapping are subsequently used to compute ρbulk and ρtap, respectively2.

113

Triplicate measurements were performed.

114 115 116

Particle flowability can be characterized by Carr’s Compressibility Index (CI) which relates to ρbulk and ρtap based on the equation:

ρ −ρ  bulk  ×100% CI =  tap ρ   tap

(1)

117 118

Crystalline structure

119

The crystalline structure of the HA carriers are determined using X-ray diffraction (XRD).

120

A thinner layer of powder samples are placed into a sample holder. It is then inserted into a

121

LabX-Shimadzu XRD6000 diffractometer (Shimadzu Corporation, Kyoto, Japan) with Cu Kα as 6

ACS Paragon Plus Environment

Page 7 of 28

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Industrial & Engineering Chemistry Research

122

X-ray source (λ = 1.5406 Å). The parameters are fixed at a scan rate of 0.5/min, voltage of 40

123

kV, current of 40 mA and step size of 0.02 for all measurements.

124 125

Moisture content

126

Thermogravimetric analysis (TGA, Simultaneous TGA/DSC SDT Q600, TA Instrument,

127

Instrument Research) is conducted to measure the moisture absorbed on the surface of particles.

128

TGA measurements are performed from 30ºC to 130ºC at a heating rate of 10ºC/min under

129

nitrogen atmosphere with 8 – 10 mg of each sample.

130 131

Specific surface area

132

The BET surface area of each HA carrier is determined. The Autosorb® Degasser

133

(Quantachrome Instruments, FL, USA) is used to dry the samples at 90ºC for 24h under nitrogen.

134

The surface area of the each sample is then measured in an Autosorb® 6B (Quantachrome

135

Instruments, FL, USA) surface analyzer using nitrogen adsorption method.

136 137

Blending of carriers with Bd

138

Budesonide (Bd) (Sigma, Singapore) is used as the model drug in the current study. The

139

Bd drug particles had a D50 of 2.8 µm and were used as received. A 100 mg mixture of carrier

140

and drug in a ratio of 10:1 by weight is mixed in a REAX top mixer (Heidolph, Kelheim,

141

Germany). Each blend is blended under 1000 rpm for 15 min.

142 143

Drug content and content uniformity

7

ACS Paragon Plus Environment

Industrial & Engineering Chemistry Research

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

144

Average drug content and content uniformity are examined by measuring the quantity of

145

Bd in the blend. 5 mg of each blend is randomly taken and dissolved into a fixed amount of

146

solvent, comprises of a mixture of 2 % nitric acid (Fluka, Singapore) with ethanol (Merck,

147

Singapore) in a volume ratio of 3:1. The solution is then analyzed using a UV spectrophotometer

148

(Shimadzu, Japan, Nottingham, UK) with a wavelength of 250 nm. The measurement is

149

performed in triplicate for all blends. The content uniformity for the mixture is assessed from the

150

coefficient of variance (CV). The CV is defined as the ratio of the standard deviation of the drug

151

content to the average drug content in the samples as percentage.

152 153

In Vitro Aerosolization and Deposition Properties

154

An eight–stage Anderson Cascade Impactor (ACI) (Copley Scientific, Nottingham, UK) is

155

used to characterize the in vitro aerosolization and deposition properties of Budesonide (Bd,

156

Sigma, Singapore) blended with the pollen-shape carriers. Rotahaler® is used as the inhaler

157

device. A schematic diagram of the ACI setup is shown in Fig. 1. For each run of the experiment,

158

8 mL of solvent containing ethanol and nitric acid is poured into the pre-separator. The impactor

159

plate of each stage is coated with 1% (w/v) solution of silicon oil in hexane to prevent bouncing

160

and re-entrainment of particles. 10 ± 0.5 mg of each blend is loaded into a hard gelatin capsule

161

(Gelatin Embedding Capsules, size 4, 0.25 cm3, Polysciences, Inc., PA) before putting into the

162

inhaler. An actuation time of 8 seconds and 4 seconds is used for air flow rate of 30 L/min and

163

60 L/min, respectively to completely disperse all the particles in the capsule. Each experimental

164

condition is repeated a minimum of three times to ensure repeatability.

165

At the end of each run, particles remained in the capsule, the inhaler and different stages of

166

the ACI are extracted. A solvent mixture of 2% nitric acid (Fluka, Singapore) with ethanol

8

ACS Paragon Plus Environment

Page 8 of 28

Page 9 of 28

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Industrial & Engineering Chemistry Research

167

(Merck, Singapore) in a volume ratio of 3:1 is used to extract the Bd. The concentration of the

168

Bd in the solvent is measured using a UV spectrophotometer (Shimadzu, Japan, Nottingham,

169

UK) with a wavelength of 250 nm. Each solution is analyzed three times and the average is

170

computed.

171

The in vitro aerosolization and deposition properties of the blend can be characterized by

172

the emitted dose (ED) and fine particle fraction (FPF). ED is the mass percentage of the drug that

173

is delivered from the inhaler and FPF is the mass percentage of the drug particles whose

174

aerodynamic diameter is smaller than 5.8 µm classified by the different stages of the ACI.

175 176

Results and discussions

177

Physical characteristics of surface modified pollen-shape HA carriers

178

For simplicity, the original unmodified HA carriers is denoted as “HA-original”. The HA

179

carriers modified by the surface etching technique is denoted as “HA-30”, “HA-40”, etc, where

180

the number represents the surface etching temperature. The SEM images of the original and the

181

surface modified HA carriers are shown in Fig. 2. It can be seen from Fig. 2(a) that HA-original

182

particles are spherical and have pollen-shape surface with dense petal-like structures. A

183

comparison of Figs. 2(a) and 1(b) indicates that a surface etching temperature of 30ºC does not

184

provide any noticeable change in the pollen-shape surface. On the other hand, Fig. 2(e) shows

185

that a surface etching temperature of 60ºC destroyed the pollen-shape surface and the particle

186

becomes irregularly shaped. As shown in Fig. 2(c), a surface etching temperature of 40ºC retains

187

the pollen-shape morphology but the petal-like structure becomes less dense. This is attributed to

188

a successful surface etching of the phosphate content present in the HA-original particles and

189

leads to a reduction in the petal-like structure of the resulting HA-40 particles. At a higher

9

ACS Paragon Plus Environment

Industrial & Engineering Chemistry Research

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

190

surface etching temperature of 50ºC, a number of fibrous structures are formed on top of the

191

petal-like structures of HA-50 particles shown in Fig. 2(d). However, the high degree of surface

192

etching causes a certain degree of deformation from the round overall particle structure. Since

193

surface etching temperatures of 40ºC and 50ºC are able to give sufficient structural change to the

194

pollen-shape surface and still maintain the overall shape of the particles. Therefore, only HA-40

195

and HA-50 carriers are used for further investigations. It is also important to note that there is no

196

obvious change in the particle size before and after surface modification. The differences

197

observed for the carrier performance can be considered a result of surface morphology alone.

Page 10 of 28

198

One important particle characteristic for DPI is the particle flowability. It directly impacts

199

the dose uniformity. A poor particle flowability leads to irregular flow and causes a large

200

variation in the amount of particles released from the capsule20. The CI index can be used to

201

characterize the particle flowability and can be calculated from ρtap and ρbulk. A high CI index

202

indicates poor flowability based on the concept that compressible and poorly flowable particles

203

are more cohesive and thus a large difference between ρtap and ρbulk. ρtap, ρbulk and CI of the HA

204

carriers before and after surface modification and their respective particle size distribution and

205

specific surface areas are shown in Table 1. It can be seen that the surface etching treatment

206

increases both ρtap and ρbulk. Through surface etching, there is a reduction in the surface density

207

of the petal-like structure. It allows the particles to be more tightly packed even in a loose

208

packing condition. Therefore, an increase in ρbulk and ρtap is observed. For HA-50, the particles

209

deviate from a round overall structure and further increases ρbulk and ρtap. However, the degree of

210

increase in ρtap and ρbulk are not at all the same. As the surface density of the petal-like structure

211

decreases, there is a reduction in the particle-particle contact and subsequently reduces the

212

cohesive nature of the particles. As shown in Table 1, HA-40 has a CI value of 39.6% and HA-

10

ACS Paragon Plus Environment

Page 11 of 28

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Industrial & Engineering Chemistry Research

213

50 has a CI value of 32.9%. This indicates that surface etching is effective in reducing the

214

particle cohesiveness and improves the particle flowability.

215

Moisture can affect particle dispersion and flowability by enhancing the particle

216

aggregation tendency. TGA is therefore carried out to measure the moisture content. The

217

thermogram showed a negligible amount of free water in all samples by expressing the marginal