Synthesis and Characterization of Dodecanethiol-Capped Cadmium

Nagaraj Patil , Saswati Ghosh Roy , Ujjal Haldar , and Priyadarsi De ... Vijila Kalarivalappil , Steven J. Hinder , Suresh C. Pillai , V. Kumar , Baij...
0 downloads 0 Views 88KB Size
Langmuir 2002, 18, 8237-8240

8237

Notes Synthesis and Characterization of Dodecanethiol-Capped Cadmium Sulfide Nanoparticles in a Winsor II Microemulsion of Diethyl Ether/AOT/Water R. B. Khomane,† Abhijit Manna,† A. B. Mandale,‡ and B. D. Kulkarni*,† Chemical Engineering Division, and Materials Chemistry Division, National Chemical Laboratory, Pune 411 008, India Received October 17, 2001. In Final Form: July 10, 2002

Introduction Synthesis of nanometer size particles of metals and semiconductors has gained considerable interest due to their novel size-dependent physicochemical and optoelectronic properties. These novel properties arise due to the large number of surface atoms (high surface-to-volume ratio) and/or the three-dimensional (3D) confinement of electrons. When the electrons and holes are confined within the three-dimensional potential well, the continuum of the states in the conduction and valance bands is broken down into discrete states with an energy spacing, relative to band edge, which is approximately inversely proportional to the square of the particle size.1 Altering the size of the particle changes the degree of confinement of the electrons and tunes the electronic structure of the solid (particularly “band edges”). These nanomaterials have found promising applications in various fields such as in microelectronic systems2,3 (light-emitting diodes and photovoltaic cells), photocatalysis,4,5 electroluminescence,6 reprography,7 and so forth. “Water-in-oil” (w/o) microemulsions consist of nanometer size water droplets dispersed in a continuous oil phase and stabilized by surfactant molecules. The reverse micellar systems are heterogeneous on a molecular scale and are thermodynamically stable and transparent. They provide a suitable reaction medium for the synthesis of nanoparticles, since water droplets represent nanoreactors where the formation of small crystallites with a narrow size distribution will be favored.8 In addition to singlephase reverse microemulsions, several phase equilibria such as Winsor I (W I), Winsor II (W II), Winsor III (W III), and Winsor IV (W IV) systems are known.9 Recently, * To whom correspondence should be addressed. Telephone/ Fax: (+91) (20) 5893095/5893041. E-mail: [email protected]. † Chemical Engineering Division. ‡ Materials Chemistry Division. (1) Schmid, G. Chem. Rev. 1992, 92, 1709. (2) Colvin, V. L.; Schlamp, M. C.; Alivisatos, A. P. Nature 1994, 370, 354-357. (3) Shim, M.; Guyot-Sionnest, P. Nature 2000, 407, 981-983. (4) Beydoun, D.; Amal, R.; Low, G.; McEvoy, S. J. Nanopart. Res. 1999, 1, 439-458. (5) Thurston, T. R.; Wilcoxin, J. P. J Phys. Chem. B 1999, 103, 1117. (6) Mattoussi, H.; Radzilowski, L. H.; Dabbousi, B. O.; Thomas, E. L.; Bawendi, M. G.; Rubner, M. F. J. Appl. Phys. 1998, 83, 7965-7974. (7) Hamilton, J. F.; Baetzold, R. C. Science 1979, 205, 1213-1220. (8) Pileni, M. P. Langmuir 1997, 13, 3266-3276.

Manna et al. have synthesized dodecanethiol-capped silver and gold nanoparticles in a Winsor II microemulsion.10 Brust et al.11 first reported the use of a two-phase method wherein the metal ions were transferred to the organic layer using a phase transfer reagent and thereafter reduced in the organic medium in the presence of suitable capping agents. Weller and his co-workers have also prepared different sizes of nanoparticles of CdS using dilute solutions (∼10-3 M) of cadmium salts and studied their adsorption and fluorescence behavior.12 Sarathy et al.13 have demonstrated that colloidal gold, platinum, and silver particles synthesized in aqueous media may be transferred into a hydrocarbon environment such as toluene by acid-facilitated coordination of the particles with alkanethiols present in toluene. The serious drawback of this method is the requirement of a relatively large quantity of concentrated HCl. Very recently, Kumar et al.14 have synthesized octadecanethiol-capped CdS nanoparticles in a biphasic liquid-liquid system in the presence of excess (>20 times) octadecanethiol. The system may be suitable for very low salt (10-4 M) concentrations. In this note, we demonstrate a new method for the synthesis of dodecanethiol- capped cadmium sulfide nanoparticles in a Winsor II microemulsion of AOT/diethyl ether/H2O. Sodium bis(2-ethylhexyl) sulfosuccinate, CH3(CH2)3CH(C2H5)CH2O2CCH2CH(SO3Na)CO2CH2CH(C2H5)(CH2)3CH3, commercially known as AOT, is a double-tailed anionic surfactant. The critical micelle concentration (cmc) value of AOT is 0.0025 M. It is known to form spherical, nanometer sized, molecular aggregates in a variety of nonpolar organic solvents. The solubility and micelle-forming ability of AOT are well established. We prefer AOT as an anionic surfactant due to its higher solubility in the organic phase (diethyl ether). Further, the anionic polar headgroups help to extract metal cations from the aqueous to the reverse micellar phase. The metal ions concentrated in the reverse microdroplets can be capped by dodecanethiol present in the system. The nanoparticles so prepared have been characterized by Fourier transform infrared (FT-IR) spectroscopy, transmission electron microscopy (TEM), X-ray photoelectron spectroscopy (XPS), and UV-visible spectroscopy to reveal the nature of thiol-capped cadmium sulfide. Most of the conventional synthesis methods deal with very dilute salt concentrations. The Winsor (W II) type system offers the possibility to use far higher (a few tens to a hundred times) salt concentrations than that of the conventional systems. It is therefore expected that the (9) Lattes, A.; Rico, I.; de Savignac, A.; Samii, A. Tetrahedron 1987, 43, 1725. (10) Manna, A.; Kulkarni, B. D.; Bandyopadhyay, K.; Vijayamohanan, K. Chem. Mater. 1997, 9, 3032-3036. (11) Brust, M.; Walker, M.; Bethell, D.; Schiffrin, D. J.; Whyman, R. J. J. Chem. Soc., Chem. Commun. 1994, 801-802. (12) (a) Resch, U.; Eychmueller, A.; Haase, M.; Weller, H. Langmuir 1992, 8, 2215. (b) Vossmeyer, T.; Katsikas, L.; Giersig, M.; Popovic, I. G.; Diesner, K.; Chemseddine, A.; Eychmueller, A.; Weller, H. J. Phys. Chem. 1994, 98, 7665. (13) Sarathy, K. V.; Thomas, P. J.; Kulkarni, G. U.; Rao, C. N. R. J. Phys. Chem. B 1999, 103, 3399-3401. (14) Kumar, A.; Mandale, A. B.; Sastry, M. Langmuir 2000, 16, 92999302.

10.1021/la011567b CCC: $22.00 © 2002 American Chemical Society Published on Web 09/07/2002

8238

Langmuir, Vol. 18, No. 21, 2002

Notes

Figure 1. FT-IR spectra of (a) free dodecanethiol and (b) nanoparticles. The KBr technique is used for recording of these spectra.

system will be useful in large-scale synthesis of CdS nanoparticles.

Table 1. FT-IR Bands for Free Thiol and Nanoparticles band position in cm-1

Experimental Section

assignment

free thiola

CdS nanoparticles

Nanoscale dodecanethiol-capped cadmium sulfide particles were prepared using a Winsor II microemulsion system. Twenty cubic centimeters of aqueous salt solution [[Cd (NO3)2], 0.04 mol dm-3] and 80 mL of 0.05 mol dm-3 AOT solution in diethyl ether were mixed together and stirred vigorously for 30 min. Next, 90 mg of dodecanethiol (4.45 × 10-4 mol) was then added to the rapidly stirring microemulsion for 10 min and allowed to stand. Next, 20 mL of 0.04 mol dm-3 aqueous sodium sulfide (Na2S‚ 9H2O) solution was slowly added to the mixture with vigorous stirring for 1 h to complete the reaction. The yellow reverse micellar phase containing the precipitate was in equilibrium with a clear aqueous phase, and this aqueous phase was separated. The solvent was removed under reduced pressure with a rotary evaporator, and the resulting sample was thoroughly rinsed with ethanol to remove adsorbed AOT, excess thiols, and other reaction byproducts. The particles so obtained were soluble in solvents such as n-hexane, n-heptane, toluene, tetrahydrofuran, and so forth.

CH2 antisymmetric stretching CH2 symmetric stretching CH2 scissoring CH3 bending (U type) CH2 twisting, wagging, and rocking

2925 (s) 2855 (s) 1465 (m) 1375 (w) 1187 (w)

2923 (s) 2852 (s) 1462 (m) 1379 (w) 1185 (sh) 1222 (m) 1043 (m) 723 (w) 620 (w)

Results and Discussion Figure 1 shows a comparison of the FT-IR spectra (4000-400 cm-1) for (a) the free thiol and (b) the composite nanoparticles. The FT-IR spectra were recorded on a Perkin-Elmer 16PC FT-IR instrument, using KBr pellets. The band positions and their assignments are listed in Table 1. The figure clearly shows that all the important bands of the pure dodecanethiol (Figure 1a) are also seen in the composite nanoparticles (Figure 1b). The commonality of the features confirms the presence of thiol as an

1044 (m) 725 (w) 620 (w)

essential component of the nanoparticles. Slight shifts were observed for CH2 antisymmetric stretching (29252923 cm-1) and CH2 symmetric stretching (2855-2852 cm-1) bands, indicating the trans conformation of the alkyl chain of adsorbed thiol molecules. A decrease in intensity of the asymmetric bending vibration of the methyl group (δsaCH3) at around 1462 cm-1 is due to capping. Figure 1 also shows the band assigned to the symmetric bending vibration (δsCH3) at around 1379 cm-1, and C-C twisting, wagging, and rocking vibrations in the broad region of 1200-800 cm-1 are much stronger (Figure 1b). The increase in intensities and more sharp nature of the spectra can be assigned to the capping effect. The XPS signals (Figure 2a,b) show the presence of principle S 2p and Cd 3d core levels in the composite particles synthesized in the Winsor II microemulsion system. XPS measurements were made using a V. G. Scientific ESCA-3000 spectrometer fitted with a separate sample preparation chamber. The absence of an XPS signal

Notes

Langmuir, Vol. 18, No. 21, 2002 8239

Figure 3. Transmission electron micrograph of thiol-capped CdS nanoparticles.

Figure 4. Histogram of the particle size distribution corresponding to the micrograph given in Figure 3.

Figure 2. XPS spectra of the nanoparticles showing (a) the Cd 3d5/2 and Cd 3d3/2 doublet with binding energies of 405.1 and 412.2 eV, respectively, and (b) S 2p.

in the binding energy (BE) region between 166 and 169 kV provides evidence of the absence of impurities (surfactant). It is clear from the high-resolution spectrum of the Cd 3d core level (Figure 2a) that there are two chemically distinct species in the spectrum, and they have been individually fit to the 3d spin-orbit components as shown in the figure. The Cd 3d5/2 peak at 406.1 eV and the Cd 3d3/2 peak at 412.86 eV are in good agreement with the published results.16 Figure 2b, over the range 158-166 eV, reveals two peaks in the S 2p core level spectrum of the nanoparticle with the peak of the S 2p3/2 BEs at 162.06 eV and 2p5/2 at 163.67 eV. These BE values are in excellent agreement with published values for the S 2p signal from self-assembled monolayers of alkanethiols on CdS nanoparticles.15,16 Thus, the XPS analysis of the material is consistent with dodecanethiol-stabilized CdS nanoparticles. Figure 3 shows the transmission electron micrograph (recorded with a TEM unit Philips EM 301) of thiol-capped CdS particles prepared in the Winsor II type microemulsion of diethyl ether/AOT/water. The sample for the (15) Terrill, R. H.; et al. J. Am. Chem. Soc. 1995, 117, 12537-12548. (16) Kundu, A.; Khosravi, A. A.; Kulkarni, S. K.; Singh, P. J. Mater. Sci. 1997, 32, 245-258.

Figure 5. UV-vis spectrum of the thiol-capped CdS nanoparticles redispersed in the n-hexane solvent.

transmission electron microscope was prepared by evaporating a drop of dilute n-hexane solution of the particles onto an amorphous carbon-coated copper TEM grid. It can be seen from this figure that all particles are nearly monodisperse and almost spherical. The TEM micrograph also shows that the particles taking part in the formation of the nanostructure maintain their distinct character and do not agglomerate into large clusters. Figure 4 shows the particle size distribution histogram for the corresponding TEM micrograph given in Figure 3. The histogram shows that more than 55% of the particles possess a diameter of 4 nm. Figure 5 shows the UV-visible spectrum of the dodecanethiol-capped CdS nanoparticles redispersed in n-hexane solvent. A Perkin-Elmer Lambda 3B doublebeam UV-vis absorption spectrophotometer was used for the recording of the UV-vis absorption of the

8240

Langmuir, Vol. 18, No. 21, 2002

dodecanethiol-capped CdS nanoparticle dispersion in the micellar phase and dispersed in n-hexane. The absorption occurs at ca. 425 nm. This peak is due to the surface plasmon absorption of the CdS nanoparticles. Elemental analysis (recorded with a Carlo Erba Instrument, model EA 1108, with a C, H, N, S, O elemental analyzer) of the thiol-capped cluster compound for C, H, and S gave values of 24.25, 4.44, and 16.43, respectively. The atomic percentages of C, H, and S work out to be 63.44, 9.87, and 36.44. The percentages of C and H gave the values of (considering the total atomic weight percent of carbon and hydrogen to be equal to 100%) C ) 84. 61% and H ) 15.38%, which are consistent with the literature reports. Thus, atomic weight percentages of C and H found in the elemental analysis are in close agreement with the composition of the dodecane chain of a thiol molecule, which supports the encapsulation. The excess atomic percentage of S present (based the theoretical value of the same in dodecanethiol) in the composite material was also calculated. We found that ∼20.6 wt % of S is present in

Notes

excess. The contribution of this excess S is from the CdS particles. In conclusion, the dual role of the anionic surfactant, viz., forming the microemulsion and facilitating the extraction of oppositely charged ions from the aqueous to the organic reverse micellar phase, has been successfully used for the synthesis of dodecanethiol-capped cadmium sulfide (CdS) nanoparticles in a Winsor II type microemulsion. A number of instrumental techniques have been used to characterize and confirm the nanoparticles. The Winsor type II system, as shown here, provides the possibility for use in large-scale synthesis of CdS nanoparticles. Acknowledgment. The authors thank Mr. R. G. Gonnade for the TEM analysis. R.B.K. thanks the Council of Scientific and Industrial Research (CSIR), Government of India, for a research fellowship. LA011567B