Tailored Chemical Properties of 4-Arm Star ... - ACS Publications

Mar 27, 2017 - Herein, we have tailored the cell adhesive properties of star shaped poly(D,L-lactide) (ss-PDLLA) by grafting gelatin to their 4 arms. ...
1 downloads 0 Views 12MB Size
Subscriber access provided by UB + Fachbibliothek Chemie | (FU-Bibliothekssystem)

Article

Tailored Chemical Properties of 4 arm star shaped poly(D,LLactide) as Cell Adhesive Three-Dimensional Scaffolds Chelladurai Karthikeyan Balavigneswaran, Sanjeev Kumar Mahto, Subia Bano, Arumugam Prabhakar, Kheyanath Mitra, Vivek Rao, Munia Ganguli, Biswajit Ray, Pralay Maiti, and Nira Misra Bioconjugate Chem., Just Accepted Manuscript • DOI: 10.1021/acs.bioconjchem.7b00071 • Publication Date (Web): 27 Mar 2017 Downloaded from http://pubs.acs.org on March 28, 2017

Just Accepted “Just Accepted” manuscripts have been peer-reviewed and accepted for publication. They are posted online prior to technical editing, formatting for publication and author proofing. The American Chemical Society provides “Just Accepted” as a free service to the research community to expedite the dissemination of scientific material as soon as possible after acceptance. “Just Accepted” manuscripts appear in full in PDF format accompanied by an HTML abstract. “Just Accepted” manuscripts have been fully peer reviewed, but should not be considered the official version of record. They are accessible to all readers and citable by the Digital Object Identifier (DOI®). “Just Accepted” is an optional service offered to authors. Therefore, the “Just Accepted” Web site may not include all articles that will be published in the journal. After a manuscript is technically edited and formatted, it will be removed from the “Just Accepted” Web site and published as an ASAP article. Note that technical editing may introduce minor changes to the manuscript text and/or graphics which could affect content, and all legal disclaimers and ethical guidelines that apply to the journal pertain. ACS cannot be held responsible for errors or consequences arising from the use of information contained in these “Just Accepted” manuscripts.

Bioconjugate Chemistry is published by the American Chemical Society. 1155 Sixteenth Street N.W., Washington, DC 20036 Published by American Chemical Society. Copyright © American Chemical Society. However, no copyright claim is made to original U.S. Government works, or works produced by employees of any Commonwealth realm Crown government in the course of their duties.

Page 1 of 43

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Bioconjugate Chemistry

1

Tailored Chemical Properties of 4 arm star

2

shaped poly(D,L-Lactide) as Cell Adhesive

3

Three-Dimensional Scaffolds

4

Chelladurai Karthikeyan Balavigneswaran,† Sanjeev Kumar Mahto,‡ Subia Bano,§

5

Arumugam Prabhakar,§,ǁ Kheyanath Mitra,ǂ Vivek Rao,§,ǁ Munia Ganguli,§,ǁ Biswajit Ray,ǂ

6

Pralay Maiti,┴ and Nira Misra*†

7 8 9 10 11 12 13 14 15 16 17



Polymer Engineering Laboratory, School of Biomedical Engineering, Indian Institute of

Technology (Banaras Hindu University), Varanasi-221005, India ‡

Tissue Engineering and Biomicrofluidics Laboratory, School of Biomedical Engineering,

Indian Institute of Technology (Banaras Hindu University), Varanasi-221005, India §

CSIR-Institute of Genomics and Integrative Biology, Mathura road, New Delhi - 110025,

India ǁ

Academy of Scientific and Innovative Research (AcSIR), Anusandhan Bhavan, 2 Rafi Marg,

New Delhi – 110001 ǂ

Department of Chemistry, Institute of Science, Banaras Hindu University (BHU), Varanasi-

221005, India ┴

School of Materials Science and Technology,, Indian Institute of Technology (BHU),

18

Varanasi-221005, India

19

E.mail : [email protected]

20 21 22 23 24 25 1

ACS Paragon Plus Environment

Bioconjugate Chemistry

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 2 of 43

26

Abstract

27

Biodegradable poly(lactic acid) (PLA) is widely used to fabricate 3D scaffolds for tissue

28

regeneration. However, PLA lacks cell adhering functional moieties, which limit its

29

successful application in tissue engineering. Herein, we have tailored the cell adhesive

30

properties of star shaped poly(D,L-Lactide) (ss-PDLLA) by grafting gelatin to their 4 arms.

31

Grafting of gelatin on PDLLA backbone was confirmed by 1H NMR and FTIR. The

32

synthesized star shaped poly(D,L-Lactide)-b-Gelatin (ss-pLG) exhibited enhanced wettability

33

and protein adsorption. The modification also facilitated better cell adhesion and proliferation

34

on their respective polymer coated 2D substrates, compared to their respective unmodified ss-

35

PDLLA. Further, 3D scaffolds were fabricated from gelatin grafted and unmodified

36

polymers. The fabricated scaffolds were shown to be cytocompatible to 3T3-L1 cells and

37

heamocompatible to Red Blood Cells (RBCs). Cell proliferation was increased upto 2.5 folds

38

in ss-pLG scaffolds compared to ss-PDLLA scaffolds. Furthermore, a significant increase in

39

cell number reveals, high degree of infiltration of cells into the scaffolds, forming a viable

40

and healthy 3D interconnected cell community. In addition to that, burst release of docetaxal

41

(DTX) was observed from ss-pLG scaffolds. Hence, this new system of grafting polymers

42

followed by fabricating 3D scaffolds could be utilized as a successful approach in variety of

43

applications where cells containing depots are used.

44

Key words

45

Ring opening polymerization, Carbodimide Chemistry, Poly (D,L-Lactide), Gelatin, 3D

46

scaffolds, Cell Depots

47

48 2

ACS Paragon Plus Environment

Page 3 of 43

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Bioconjugate Chemistry

49

INTRODUCTION

50

The ultimate goal of an artificial 3D scaffold is to mimic the natural extracellular

51

environment of cells for successful tissue regeneration. Over the past few years, researchers

52

have been strongly focusing on studies related to cell-material interactions to understand the

53

cellular functions and behaviour in response to the materials1. Such materials initially serve

54

as a physical support for the cells to facilitate adhesion followed by manifestation of

55

subsequent cellular functions, including proliferation, migration and differentiation

56

Plethora of literatures is available on biodegradable polymers with an increasing research

57

effort particularly in the last ten years. Yet there has been no corresponding rise in their final

58

commercial end products useful for tissue regeneration4 indicating, cell-material interface

59

science needs more attention towards developing such novel biomaterials in a better and

60

efficient way. Therefore, cell − material interface science needs more attention towards

61

developing novel biomaterials that meets the industrial demands. Therefore, designing a

62

scaffold to control the cell-material interactions could be highly important for the successful

63

development of 3D matrix for tissue engineering applications.

64

Synthetic biodegradable polymer poly(lactic acid) (PLA) is widely used to fabricate 3D

65

scaffolds for tissue regeneration due to their biodegradable nature, good mechanical

66

properties, and importantly their FDA approval for its clinical use. 4 arm star shaped PLA

67

representing one of the branched structures of PLA,4 exhibits various important properties of

68

tissue engineering scaffolds such as chemical multifunctionality 5, low viscosity6 and higher

69

degradation rate7, 8 compared to their linear counterpart. However, the hydrophobic nature of

70

PLA surface does not promote cell adhesion thereby hampering its applications in tissue

71

engineering9. Initial response of the cells to the scaffold is dependent on the surface

72

properties since material’s surface is the first site of cellular contact. Thus, the ability of

2, 3

.

3

ACS Paragon Plus Environment

Bioconjugate Chemistry

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 4 of 43

73

supporting cell adhesion is the prerequisite for any material to serve as the tissue engineering

74

scaffold. In a natural environment, cell-membrane interaction occurs through integrin binding

75

sequences of ECM proteins, including RGD, YIGSR, REDV, etc10. Therefore, immobilizing

76

adhesive ECM proteins such as fibronectin, laminin and their functional putative peptides

77

(Arg-Gly-Asp (RGD) and Tyr-Ile-GlySer-Arg (YIGSR)) as well as other biocompatible

78

molecules including gelatin and chitosan to the surface of materials is considered to be an

79

innovative approach to control cell adhesion11, 12.

80

Many surface-modification techniques have been reported to enhance the biocompatibility

81

and cellular properties of PLA, that include polymerization grafting13, 14, ozone oxidization15,

82

plasma modification16,

83

aminolysis,13,

84

modification onto PLA substrates has been reported by photografting, surface initiated Atom

85

Transfer Radical Polymerization (ATRP) based chemical grafting and plasma treatment23-25.

86

All such modifications are usually done after the fabrication of either films or scaffolds. To

87

the best of our knowledge very few articles report the scaffold fabrication using copolymers

88

of RGD / RGD mimicking peptides coupled biodegradable polymers such as PLA and PCLA

89

(poly(3-caprolactone-co-lactide))26, 27. Here, we have assessed a hypothesis that 3D scaffolds

90

fabricated from gelatin grafted 4 arm star shaped poly(D,L-Lactide) (ss-PDLLA) copolymer

91

may support the cell growth and proliferation more appropriately, as explained in Figure 1.

92

In particular, cells can migrate deep into the fabricated 3D scaffolds and form the 3D

93

interconnected cell community; whereas such interconnected cell community is highly

94

unlikely to be achieved through other surface modification techniques. As of now, no such

95

study has been reported for controlling the cell adhesion by gelatin grafted on ss-PDLLA(

96

star-shaped PDLLA-b-Gelatin (ss-pLG)).

17

, physical entrapment of cell adhering molecules18, hydrolysis,19,

19

, surface coating20 and layer-by-layer self-assembly21,

22

. Notably, gelatin

4

ACS Paragon Plus Environment

Page 5 of 43

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Bioconjugate Chemistry

97 98 99 100 101 102 103 104 105 106

Figure 1 Schematic representation of cell proliferation within the surface treated scaffolds and the scaffolds fabricated from gelatin grafted polymers. In case of surface-treated 3D scaffolds, it is likely that distribution of modified entities will be largely non-uniform throughout the scaffold. In such scenarios, introduction of treating moieties is generally found hindered towards the core region of the scaffold. Whereas in case of 3D scaffolds fabricated from gelatin coupled polymers, gelatin is expected to be present in situ within the entire region of the scaffold uniformly since it is already grafted with the backbone of PDLLA. Thus, the fabricated scaffolds are thought to facilitate interconnected 3D cellular networks throughout the matrix.

107

In the present study, tailoring the chemical properties of star shaped PDLLA (ss-PDLLA) by

108

gelatin grafting and their ability of supporting cellular growth on the modified polymers is

109

demonstrated. It is known that one can control the wettability of PLA by branching

110

coupling it with some hydrophilic polymers such as poly(ethylene glycol)29, poly(N-

111

vinylpyrrolidone)30, 31, gelatin12, 23, etc through chemical reactions. As a result, PLA can be

112

tuned preferentially from super-hydrophobic to moderately hydrophilic. We used gelatin (a

113

denatured protein of collagen that has the integrin binding receptor such as DGEA32), for

114

modulating the wettability and cell adhesion behaviour of ss-PDLLA polymers. Therefore,

28

and

5

ACS Paragon Plus Environment

Bioconjugate Chemistry

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 6 of 43

115

herein we report the synthesis and characterization of ss-PDLLA and ss-pLG, followed by

116

fabricating them into 3D scaffolds by freeze drying technique. Considering the advantage of

117

hydrophilicity after gelatin grafting to different arms of PDLLA, we propose that ss-pLG

118

could be a versatile platform for the proliferation of cells in 3D environment with tuneable

119

cellular behaviour and responses. In order to evaluate our hypothesis and to use our ss-pLG

120

scaffolds for tissue engineering applications, we cultured 3T3-L1 cells on ss-pLG polymeric

121

scaffold; unmodified ss-PDLLA scaffold was used for the comparative study. We observed

122

that ss-pLG polymeric scaffolds prominently modulated the cell adhesion property.

123

Therefore, such tuning of cellular compatibility properties of polymers synthesized by simple

124

chemical reactions of gelatin grafting will certainly be useful for 3D culturing of cells,

125

especially required in various tissue engineering applications.

126

RESULTS AND DISCUSSION

127

Synthesis and characterization of gelatin grafted copolymer (ss-PDLLA-b-Gelatin)

128

Methods for the synthesis of ss-PDLLA followed by ss-pLG are shown in Scheme 1, where

129

we used combined ring opening polymerization (ROP) followed by end functionalization of

130

gelatin by carbodimide chemistry. Initially, 4 arm ss-PDLLA was synthesized via our earlier

131

reported method,31 where ROP of D,L-Lactide was done in bulk at 150ᵒC using

132

pentaerythritol as initiator and Sn(Oct)2 as catalyst with the molar feed ratio of D,L-Lactide

133

to pentaerythritol at 693.3. The 1H NMR confirms its formation; Mn (NMR) and conversion

134

(NMR) was found to be 1,86,300 g mol-1 and 97.2% respectively (Figure S1). Mn (GPC) and

135

Mn/Mw of the synthesized polymer calibrated against PMMA standard was 3,79,000 g mol-1

136

and 1.9 respectively (Table 1). To graft the gelatin into ss-PDLLA arm, carboxyl terminated

137

PDLLA was first synthesized by ring opening of succinic anhydride using ss-PDLLA-OH.

138

The appearance of new peaks at 3.6 (g+h) comes from the methylene protons of succinic 6

ACS Paragon Plus Environment

Page 7 of 43

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Bioconjugate Chemistry

139

anhydride and the disappearance of end terminal methine proton of ss-PDLLA at 4.36

140

confirms successful ring opening reaction (Figure 2A & Figure S1). The end terminal –

141

COOH group was activated by EDC.HCl and NHS followed by coupling with gelatin was

142

done at unit molar feed ratio of 1 (PDLLA-COOH to Gelatin). The chemical coupling was

143

confirmed by 1H NMR (Figure S1), where apart from the characteristic peaks of gelatin,

144

characteristic peaks of ss-PDLLA at 5.1-5.2 and 1.46 ppm corresponding to the backbone

145

methine and pendent methyl protons, respectively, are present (Figure 2A & Figure S1).

146

Detailed description about synthesis and conversion is given in supporting information.

147 148 149 150

Scheme 1. Synthesis of gelatin grafted star shaped PDLLA by ROP using pentaerythritol as initiator and carbodimide mediated end functionalization methods

151 152

Gelatin grafting to ss-PDLLA backbone was further analysed by FTIR spectroscopic

153

technique. Figure 2B shows the respective FTIR spectra of ss-PDLLA-COOH, gelatin and 7

ACS Paragon Plus Environment

Bioconjugate Chemistry

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 8 of 43

cm-1 which

154

ss-pLG. ss-PDLLA showed its characteristic peaks at 2998, 2939 and 1765

155

corresponds to asymmetric, symmetric stretching of CH2 and carbonyl stretching,

156

respectively33. (Figure S2). When ss-PDLLA-OH opened succinic anhydride ring,

157

characteristic shifting was found from 1765 to 1760 cm-1. Pure gelatin showed the

158

characteristic peaks at 1537 (amide II), 1661(amide I) and 3462 cm-1 for its distinct C=O

159

bond vibrations and coupling of bending of N–H bond and stretching of C–N bonds,

160

respectively

161

peaks shifted to lower frequencies at 3284 and 1627 cm-1. This observation suggests that –

162

NH2 group of gelatin has successfully coupled with the -COOH group of ss-PDLLA. ss-pLG

163

also showed the characteristic peaks of ss-PDLLA at 2916, 2851 and 1743 cm-1 which further

164

supports that ss-PDLLA backbone is present in ss-pLG polymer, whereas the intensity of

165

peak at 1743 cm-1 corresponding to the carbonyl stretch of ss-PDLLA backbone was weak. It

166

might be due to the higher content of gelatin or wrapping of ss-PDLLA by gelatin in the ss-

167

pLG

168

XPS confirmed the presence of gelatin in the ss-pLG polymer as the large increase in

169

intensity of nitrogen and the shift in the binding energy, whereas ss-PDLLA did not show any

170

peak respective for the nitrogen in XPS spectrum (Data not shown) (Figure 2C).26 Wide XPS

171

spectrum of ss-pLG scaffolds were presented in Figure S3.

172

Table 1 GPC Characteristic data star shaped PDLLA

34

. After coupling of gelatin into ss-PDLLA back bone, these amide stretching

Sample

Conversion (%)a

Mn(NMR)b

Mn(GPC)c

Mn/Mw

ss-PDLLA

97.2

1,86,300

379000

1.9

a

Conversion was determined by comparing the peak area of the residual poly(D,L-Lactide) ~ 5.1-5.2

and monomer D,L-Lactide ~ 5.3 ppm using 1H NMR

8

ACS Paragon Plus Environment

Page 9 of 43

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Bioconjugate Chemistry

b

Determined from 1H NMR by comparing the methylene proton of pentaerythritol and methine proton

of ss-PDLLA at ~ 4.2 and ~ 5.1-5.2 ppm for ss-PDLLA c

Determined by GPC (DMF, 0.5 mL/min, 40 ºC) calibrated against PMMA standards

173

9

ACS Paragon Plus Environment

Bioconjugate Chemistry

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 10 of 43

174

10

ACS Paragon Plus Environment

Page 11 of 43

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

175 176 177 178

Bioconjugate Chemistry

Figure 2. Characterization of polymers by 1H NMR, FTIR, XPS, TGA and DSC: (A) 1H NMR spectra of star shaped polymers namely ss-PDLLA-COOH, Gelatin, ss-pLG. (B) FTIR spectra of the respective series of star shaped polymers. (C) XPS spectrum of ss-pLG. (D) TGA and (E) DSC of series of star shaped polymers namely gelatin, ss-PDLLA and ss-pLG.

179

180

The thermogravimetric analysis (TGA) of ss-PDLLA, Gelatin, ss-pLG are presented in

181

Figure 2D. Thermal degradation profile of gelatin modified and unmodified polymers were

182

quite different. It can be seen that unmodified polymers ss-PDLLA and gelatin showed Tonset

183

at 241 and 285 ᵒC whereas Tmax of the polymers were found to be 300 and 457 ᵒC

184

respectively. On the other hand, the modified copolymer ss-pLG showed improved thermal

185

properties than their original unmodified polymers. Tmax of ss-pLG was found to be 455 ᵒC

186

which almost equivalent to the gelatin (Figure 2D). This thermal behaviour may be attributed

187

due to the strong coupling of gelatin onto the ss-PDLLA back bone. Moreover, ss-pLG show

188

two different distinct degradation peaks owing to the PDLLA and gelatin block. From this

189

observation, it is clear that the modified ss-pLG has better thermal stability than their

190

unmodified ss-PDLLA.

191

DSC thermograms of ss-PDLLA, gelatin and modified ss-pLG are shown in Figure 2E. In

192

second heating run, Tgs of ss-PDLLA, gelatin, and ss-pLG were observed at 30.36, 142.9, and

193

112.59 ᵒC, respectively. None of the star shaped evaluated polymers showed melting

194

endotherms or crystallization exotherms which suggests that the ss-PDLLA or gelatin

195

coupled ss-PDLLA (ss-pLG) are highly amorphous in nature. Moreover, because of the

196

grafting of gelatin into PDLLA, clear shifting of Tg was observed from 30.36 to 112.59 ᵒC for

197

ss-pLG. The observed higher shifting in ss-pLG clearly indicates the presence of higher

198

amount of gelatin in the PDLLA arm (ss-pLG).

199

Influence of gelatin grafting on protein adsorption and cell adhesion 11

ACS Paragon Plus Environment

Bioconjugate Chemistry

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 12 of 43

200

Gelatin is a natural protein that possesses inherent integrin binding sites and known for the

201

cell adhesion properties. Therefore, we demonstrate this property of gelatin by chemically

202

grafting it to star PDLLA (ss-PDLLA) backbone. Before cell culturing, effects of gelatin on

203

different polymer arms were examined for the protein adsorption efficiency. 12 % polymer

204

films were made from ss-PDLLA and ss-pLG polymers, and further evaluated for their

205

protein adsorption property. Both the films were incubated in BSA after they were wet in

206

PBS completely. ss-pLG film showed higher adsorption, which was 2.6 folds greater owing

207

to its hydrophilicity compared to ss-PDLLA (Figure 3A). It is important to note that ss-

208

PDLLA also exhibits noticeable adsorption of BSA, most likely due to its hydrophilic

209

property compared to linear PDLLA (data not shown)

210

indicate that gelatin modified PDLLA (ss-pLG) facilitate higher degree of protein adsorption

211

which is a crucial parameter required during cell culturing process.

212

In order to assess the effects of cell−material interactions as well as cell-cell interactions,

213

3T3-L1 cells were cultured on three different substrates (gelatine, ss-PDLLA and ss-pLG) at

214

low seeding densities. Typically, the focal adhesions contain transmembrane proteins i.e.

215

integrin αvβ3 as well as plaque proteins (paxillin, vinculin etc.), which connect the cells to

216

underlying substrates. Hence, determination of focal contacts can be used as an index of cell

217

adhesion strength. Vinculin is a cytoskeletal protein associated with cell-cell and cell-matrix

218

junctions. It is involved in the anchoring of filamentous actin (F-actin) to the membrane

219

adhesion molecules. To evaluate the cell adhesions associated with normal physiological

220

proteins, we chose vinculin as a model protein that was costained with actin filament and cell

221

nuclei. . Post 24 h seeding, 3T3-L1 cells cultured on polymer coated cover glass were

222

observed to be speroidal in shape and did not exhibit a proper shape of well-spread healthy

223

cells. Also, actin staining revealed the intense, mesh-like red stains extended from the cell

28, 35

(Figure 3B). These results

12

ACS Paragon Plus Environment

Page 13 of 43

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Bioconjugate Chemistry

224

perimeter; indicating the compromised status of the cells (Figure 3C). The intensified

225

vinculin expression at the edge of a cell indicated the presence of strong integrated adhesive

226

sites in case of gelatin (control) and gelatin coupled PDLLA (ss-pLG) coated cover glass.

227

Gelatin modified ss-pLG were found more effective than the unmodified polymer in terms of

228

establishing focal contacts, since the vinculin expression was clearly seen in almost all the

229

cells and also the cell shape were comparable with the gelatin coated cover glass. In contrast,

230

very weak fluorescence was observed on unmodified ss-PDLLA (Figure 3C).

231 13

ACS Paragon Plus Environment

Bioconjugate Chemistry

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

232 233 234 235 236 237 238 239 240

Page 14 of 43

Figure 3. Demonstration of cell adhesion behaviour on polymer coated 2D cover glass; (A) BSA protein adsorption on to the 2D polymer film after 4 h of incubation. Protein estimation was done by using micro BCA kit. Experiments were done in triplicate and results are expressed as mean ±SD (n=3). *p