Subscriber access provided by University of Otago Library
Communication
Deterministic switching of the growth direction of self-catalyzed GaAs nanowires Eero Koivusalo, Teemu Hakkarainen, Helder Vinicius Avanço Galeti, Yara Galvão Gobato, Vladimir G. Dubrovskii, and Mircea D. Guina Nano Lett., Just Accepted Manuscript • DOI: 10.1021/acs.nanolett.8b03365 • Publication Date (Web): 11 Dec 2018 Downloaded from http://pubs.acs.org on December 13, 2018
Just Accepted “Just Accepted” manuscripts have been peer-reviewed and accepted for publication. They are posted online prior to technical editing, formatting for publication and author proofing. The American Chemical Society provides “Just Accepted” as a service to the research community to expedite the dissemination of scientific material as soon as possible after acceptance. “Just Accepted” manuscripts appear in full in PDF format accompanied by an HTML abstract. “Just Accepted” manuscripts have been fully peer reviewed, but should not be considered the official version of record. They are citable by the Digital Object Identifier (DOI®). “Just Accepted” is an optional service offered to authors. Therefore, the “Just Accepted” Web site may not include all articles that will be published in the journal. After a manuscript is technically edited and formatted, it will be removed from the “Just Accepted” Web site and published as an ASAP article. Note that technical editing may introduce minor changes to the manuscript text and/or graphics which could affect content, and all legal disclaimers and ethical guidelines that apply to the journal pertain. ACS cannot be held responsible for errors or consequences arising from the use of information contained in these “Just Accepted” manuscripts.
is published by the American Chemical Society. 1155 Sixteenth Street N.W., Washington, DC 20036 Published by American Chemical Society. Copyright © American Chemical Society. However, no copyright claim is made to original U.S. Government works, or works produced by employees of any Commonwealth realm Crown government in the course of their duties.
Page 1 of 50 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Nano Letters
1
Deterministic switching of the growth direction of
2
self-catalyzed GaAs nanowires
3
Eero S. Koivusalo* 1, Teemu V. Hakkarainen1, Helder V. A. Galeti2, Yara G. Gobato3,
4
Vladimir G. Dubrovskii4, Mircea D. Guina1
5
1
Optoelectronics Research Centre, Tampere University of Technology, P.O. Box 692,
6 7
FIN-33101 Tampere 2
Electrical Engineering Department, Federal University of São Carlos, 13565-905, São
8 9
Carlos-SP, Brazil 3
Physics Department, Federal University of São Carlos, 13565-905, São Carlos-SP,
10 11
Brazil 4
ITMO University, Kronverkskiy prospekt 49, 197101 St. Petersburg, Russia
12
ABSTRACT: Typical vapor-liquid-solid growth of nanowires is restricted to vertical one-
13
dimensional geometry, while there is a broad interest for more complex structures in the
14
context of electronics and photonics applications. Controllable switching of the nanowire
15
growth direction opens up new horizons in the bottom-up engineering of self-assembled
16
nanostructures, for example, to fabricate interconnected nanowires used for quantum
ACS Paragon Plus Environment
1
Nano Letters 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 2 of 50
17
transport measurements. In this work, we demonstrate a robust and highly controllable
18
method for deterministic switching of the growth direction of self-catalyzed GaAs
19
nanowires. The method is based on the modification of the droplet-nanowire interface in
20
the annealing stage without any fluxes and subsequent growth in the horizontal direction
21
by a twin-mediated mechanism with indications of a novel type of interface oscillations.
22
A 100% yield of switching the nanowire growth direction from vertical to horizontal is
23
achieved by systematically optimizing the growth parameters. A kinetic model describing
24
the competition of different interface structures is introduced to explain the switching
25
mechanism and the related nanowire geometries. The model also predicts that growth of
26
similar structures is possible for all vapor-liquid-solid nanowires with commonly observed
27
truncated facets at the growth interface.
28
KEYWORDS Self-catalyzed GaAs nanowires, Growth direction, Crystal facets, Surface
29
energetics
30
Precise shaping of III-V semiconductor nanowires (NWs) is paramount for their
31
functionalization into electronic and photonic devices. In particular, GaAs/AlGaAs NW-
ACS Paragon Plus Environment
2
Page 3 of 50 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Nano Letters
32
based lasers integrated on silicon waveguides [1], monolithic LEDs [2, 3], and functional
33
NW array solar cells [4] have been the important milestones in this development. All these
34
achievements have relied on the axial or radial heterostructures within one-dimensional
35
(1D) NWs. Extension of the NW growth beyond 1D geometry provides a suitable template
36
for delicate quantum transport measurements [5, 6]. Several approaches have previously
37
been used to form a versatility of three-dimensional NW-based structures. In particular,
38
Au-catalyzed NW crosses have been grown on a (100) substrate producing rather
39
random InAs NW meshes [6], and in a more controllable way on a pre-patterned substrate
40
[7]. A ridged template covered by oxide with pre-determined nucleation sites has provided
41
another approach to grow more regular InAs
42
Interconnected NWs can also be produced by switching the NW growth direction with
43
respect to the typical [or in the case of wurtzite (WZ) NWs] direction of the
44
substrate normal. The most convenient 90° switching of the growth direction has been
45
demonstrated for Au-catalyzed WZ InAs NWs [7] and catalyst-free InAs(Sb) NWs [10]. In
46
optics and photonics, possible applications of such structures include circular dichroism
47
in the optical response of chiral nanostructures [11], exploiting the waveguiding properties
[8, 9] and InSb [5] NW crosses.
ACS Paragon Plus Environment
3
Nano Letters 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 4 of 50
48
of semiconductor NWs. [12, 13] This effect further increases the interest in controlling the
49
NW growth direction. To date, the yield of bent NWs has always been less than 100 %
50
within the framework of self-catalyzed approach. Furthermore, not all the horizontal
51
growths start in the same horizontal plane, which is unfavorable for further contacting the
52
NWs.
53
The simplest mechanism for switching the NW growth direction is driven by a catalyst
54
droplet wetting one of the NW side facets [7, 10, 14]. After that, more complex growth
55
effects may occur, including the formation of new facets or twin planes separating
56
different facets. Using these effects, even reversible switching of the growth direction has
57
been demonstrated in Au-catalyzed InP NWs [15]. In addition, twinning is known to
58
facilitate the formation of kinks and other kind of structures such as nanomembranes [16],
59
flags [14] and sails [17]. Very important information on the kinetics of kinking in Au-
60
catalyzed NWs is provided by in-situ transmission electron microscopy (TEM), as
61
descried previously [18, 19]. Despite the significant progress in understanding and
62
controlling the NW growth direction by different methods, a simple and robust procedure
63
for achieving 100% yield of horizontal self-catalyzed NW growth in one horizontal plane
ACS Paragon Plus Environment
4
Page 5 of 50 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Nano Letters
64
is still lacking. Consequently, this work reports a method to grow very regular ensembles
65
of 90° bent GaAs NWs on silicon in the self-catalyzed approach.
66
By using a lithography-free SiOx patterns as templates for the self-catalyzed vapor-
67
liquid-solid (VLS) growth, we have been able to obtain GaAs NWs with the controllable
68
number density, high quality zincblende (ZB) crystal structure and remarkable sub-
69
Poissonian length uniformity [20–22]. Here, we show that this growth method can be
70
extremely suitable to induce bent NW structures with horizontal growth. The deterministic
71
switching of the growth direction occurs in the same horizontal plane due to the narrow
72
length distribution of the initial NWs. This is highly desirable for fabrication of
73
interconnected NWs. 100% yield of regularly bent NWs is achieved simply by a growth
74
interruption, which determines a transition from vertical to horizontal growth. We
75
investigate in detail the previously unknown growth mechanism in different stages and
76
show that the NW morphology is generally sensitive to the duration of the growth
77
interruption, the local V/III ratio, and the NW diameter. Longer growth interruption is found
78
to deterministically switch the NW growth direction by 90° with a 100% yield. We develop
79
a model, which describes the observed reshaping of the growth interface and shows that
ACS Paragon Plus Environment
5
Nano Letters 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 6 of 50
80
the deterministic transition from vertical to horizontal growth upon the growth interrupt
81
must be a general phenomenon for all self-catalyzed III-V NWs under the appropriate
82
conditions. Thus, the insights presented here may help to either avoid the unwanted
83
kinking during the NW growth or deterministically switch the NW growth direction when
84
required for particular applications.
85
The self-catalyzed GaAs NWs were grown by solid source molecular beam epitaxy
86
(MBE) on lithography-free oxide pattern templates fabricated on p-Si(111) substrates via
87
droplet epitaxy. The lithography-free templates are fabricated on HF etched, oxide-free
88
Si substrates, by depositing Ga droplets on the substrate and crystallizing the droplets
89
into GaAs under the As flux. After that, the templates are oxidized in air and loaded back
90
into the MBE chamber, where the GaAs mounds are evaporated to form the lithography-
91
free oxide patterns, on which the NWs are in-situ grown, as described in [20, 22]. The
92
NWs were grown on four different templates with the nucleation site densities varying
93
from 5×107 cm-2 to 5×108 cm-2. The vertical NW growth was initiated with a 40 s pre-
94
deposition of Ga droplets, re-evaporation of the droplets and simultaneously opening the
95
Ga and As2 fluxes. The NW growth was conducted at 640 °C, as determined by
ACS Paragon Plus Environment
6
Page 7 of 50 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Nano Letters
96
pyrometer, the Ga deposition rate was 0.3 µm/h, as calibrated for (100) GaAs growth,
97
and the V/III beam equivalent pressure (BEP) ratio was 9. The vertical NW growth time
98
was 20 min, except for three samples with variable diameters for which the growth
99
durations from 20 to 30 min were used. More details on the template fabrication and the
100
NW growth method can be found in Refs. [20–22]. After growth of the vertical part, the
101
NWs were annealed for 20 to 70 s at the growth temperature without any fluxes in order
102
to reshape the droplet-NW interface. After the annealing, the NW growth was resumed
103
by simultaneously providing the Ga and As fluxes. The V/III BEP ratio for the horizontal
104
growth was varied from 7 to 11. After growth, the samples were rapidly cooled down.
105
Additional samples with vertical NWs grown for 20 min and rapidly cooled down (template
106
density 5×108 cm-2), and NWs gone through 45 s annealing (template densities 2×108 cm-
107
2,
108
fabricated as the references to study the droplet-NW interface and the NW dimensions
109
before the growth continuation.
5×108 cm-2 and 5×107 cm-2, and growth durations from 20 to 30 min) were also
110
The NW morphologies were studied using scanning electron microscopy (SEM). A
111
typical NW sample after 20 min of vertical growth and immediate cool down without any
ACS Paragon Plus Environment
7
Nano Letters 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 8 of 50
112
fluxes is shown in Figures 1 (a) and (d). It is clearly seen that the Ga droplets remain
113
stationary on the NW tips just after growth. In contrast, the sample that was annealed for
114
45 s at the growth temperature prior to cool down [Figure 1 (b) and (e)] exhibits 100%
115
yield of droplets falling toward one of the (110) side facets. When the growth is resumed
116
after annealing by simultaneously opening the Ga shutter and As valve, the NWs continue
117
their growth perpendicular to their initial growth direction [Figures 1 (c) and (f)], or slightly
118
downward [Figures 1 (c) and (g)]. Perpendicularly grown horizontal sections are referred
119
to as type 1 and downward pointing sections as type 2. The azimuthal direction of the
120
bent NW part is toward one of the directions associated with the corners of the
121
(110) sidewalls, in contrast to the droplet position after the annealing [see the top-view
122
images in Figures 1 (e) to (g)].
ACS Paragon Plus Environment
8
Page 9 of 50
(a) Self-catalyzed NW growth
(e)
Annealing
(c) Continued growth nm
1 µm
(d)
(b)
20
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Nano Letters
1 µm
(f)
1 µm Type 1
(g)
Type 2
123 124
Figure 1. Growth of bent GaAs NWs: (a) and (d) Vertical NWs grown for 20 min and rapidly cooled
125
down; (b) and (e) NWs annealed at the growth temperature for 45 s prior to cool down; (c) NWs
126
grown for 5 min after 45 s annealing; Side- and top-view images of (f) type 1 horizontal and (g)
127
type 2 downward growth. Scale bars in low magnification 30° tilted images are 1 µm in (a) to (c)
128
and 100 nm in (d) to (g).
129
To further understand the formation mechanism of these structures, the post-annealing
130
droplet-NW interfaces were analyzed by SEM and high-resolution transmission electron
ACS Paragon Plus Environment
9
Nano Letters 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 10 of 50
131
microscopy (HR-TEM) [JEOL JEM-2200FS operated at 200 kV and FEI Tecnai G2-F20
132
operated at 200 kV for Figure 4 (b)]. Two different droplet–NW interface shapes with
133
respect to the [110] zone axis (ZA) were found by TEM, as shown in Figures 2 (a) and
134
(b). The first shape is dominated by the A-polar (1-1-1) facet and the second type by the
135
(0-10) facet. The third low index facet is the B-polar (-111) facet forming below the (0-10)
136
one, as shown in Figure 2(b). Otherwise, the structures compose of minor higher index
137
facets. The facets are identified based on the assumption that the NW top facet is (-1-1-
138
1) and the NW sidewalls are (110). The growth direction is identified as B because
139
it is the common growth direction of self-catalyzed GaAs NWs [23, 24], while A-polar GaAs
140
NWs are rarely achieved and mainly using Au-catalyzed VLS growth [25, 26]. It should also be
141
noted that the radial symmetry of the NW is three-fold. This symmetry yields three
142
possible sets of [110] ZA that give equivalent results for the facet identification. The one
143
presented here is an arbitrarily chosen example showing the droplet-NW interface of a
144
particular NW.
ACS Paragon Plus Environment
10
Page 11 of 50
(a)
(b)
---
(111)
20 nm
(111)
20 nm
- -
---
(111)
(010)
-
-
(101)
--
(811)
-
(110)
-
(111)
(d) - 0) (1-0 1) (11
(- 110) 101) (
(e)
---
(111) (010) -(111)
(f)
---
--
(111)
(111) (011)
145
20 nm
(101)
(011)
50 nm
(111)
-
--
(c)
---
(100)
(011)
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Nano Letters
-
(010)
(g) 109.5°
-
(011)
(h) 125.3°
-
(101)
146
Figure 2. (a)–(c) TEM micrographs of three NWs annealed for 45 s at the growth temperature
147
prior to cool down. The ZAs marked in the micrographs are also marked in the SEM image of
148
droplet-free NW top facet in (d) and sketches (e), (g) and (h). SEM image (d) and top-view sketch
149
(e) are aligned with respect to each other. Complementary SEM analysis of (d) is presented in
150
the SI.
151
Both dominating reshaped facets are inclined toward one of the corner directions
152
of the NW sidewalls, perpendicular to the [110] ZA used for imaging. However, back-view
153
TEM [Figure 2 (c)] and top-view SEM [Figure 1 (e)] show that the droplets are tilted
154
symmetrically toward one of the (110) side facets. The shape of the NW growth interface
ACS Paragon Plus Environment
11
Nano Letters 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 12 of 50
155
was imaged by SEM after removing the Ga droplets by HCl etching. SEM analysis
156
revealed the pentagonal shape of the top facet marked by the dashed line in Figure 2 (d),
157
and that two of the sidewall corners are hidden under the reshaped facets. Based on
158
these results, the interface configurations shown in Figures 2 (a) and (b) are interpreted
159
as different views of similar structure, illustrated in the sketches in Figures 2 (e)–(h). More
160
details on the SEM analysis of the droplet-NW interface are given in the supporting
161
information (SI).
162
Results of the TEM analysis of a type 1 NW structure, shown in Figures 3 (a) and (b),
163
reveal pure ZB structure throughout the whole NW, with a single twin plane extending
164
along the horizontal section HR-TEM images in Figures 3 (c) to (e) are aligned in such a
165
way that the top side of the horizontal section is facing upward. These images show two
166
different interface configurations existing during growth of type 1 horizontal sections. Both
167
configurations are dominated by a flat (111) plane on one side of the twin plane, and
168
feature a combination of smaller facets on the other. For the NW imaged in Figure 3 (c),
169
the dominating flat (111) plane is B-polar as it is situated above the twin plane. For the
170
NW in Figure 3 (d), the dominating (111) plane is A-polar, and lies below the twin plane.
ACS Paragon Plus Environment
12
Page 13 of 50 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Nano Letters
171
This (111) A facet corresponds to the (1-1-1) plane marked in Figure 2 (a). The HR
172
magnification shown in Figure 3 (e) confirms that the (111) planes exist on both sides of
173
the twin plane. It should be noted that defect-free ZB structure without twin planes was
174
observed at the tip of all investigated NWs before and after the annealing step, as shown
175
in the SI and Figure 2, respectively. Based on these observations, we conclude that type
176
1 growth is initiated by nucleation of the twin plane which forms the (111)B plane to
177
oppose the initial (1-1-1) plane seen in Figure 2 (a). The two (111)B and (111)A opposing
178
facets pin the droplet to sustain the horizontal growth.
ACS Paragon Plus Environment
13
Nano Letters 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 14 of 50
179 180
Figure 3. HR-TEM analysis of type 1 bent GaAs NWs. The low magnification image in (a) and
181
selective area diffraction (SAED) patterns in (b) reveal the excellent crystal purity in the ZB phase,
182
and a single twin plane present in the horizontal section. Two different droplet-NW interfaces are
183
dominated by a flat (111)B plane in (c) and (111)A plane in (d). Periodic faceting of the top of the
ACS Paragon Plus Environment
14
Page 15 of 50 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Nano Letters
184
horizontal NW section can clearly be seen in (c) and (d). (e) HR magnification of the twin section
185
that features both (111)A and (111)B facets.
186
TEM analysis conducted on a type 2 NW structure reveals some similarities with type
187
1 growth. In particular, Figure 4 (a) shows that type 2 downward growth occurs on a NW
188
where a single twin is present, as we saw earlier for type 1. However, in this case the twin
189
is found in the vertical part, above the downward type 2 growth [Figure 4 (a), SAED
190
pattern 1] and is most likely formed when the growth is resumed. The downward growth
191
continues directly along the B direction [Figure 4 (b)] pointing 109° away from the
192
original NW growth direction. This is the direction of the (-111) facet marked in Figure
193
2(b). Thus, type 2 downward growth is interpreted to start with nucleation of a single twin
194
plane and the droplet sliding down from the (0-10) facet wetting the (-111) facet marked
195
in Figure 2(b), where the growth continues. During the downward growth, the (-111) facet
196
remains flat and no microfacetting in the droplet-NW interface is witnessed [Figure 4 (b)
197
and SI].
198
The NW shown in Figure 4 (a) is aligned to a [110] ZA, which is rotated by 60° around
199
the NW axis from the direct side-view [Figure 1(g)]. In this case, possible twinning of the
ACS Paragon Plus Environment
15
Nano Letters 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 16 of 50
200
downward part cannot be seen because a twin in that growth direction rotates the zone
201
axis away from the [110]. Hence, only one set of the diffraction points would be seen in
202
the SAED pattern even if the downward section were twinned. Therefore, additional TEM
203
analysis in side-view configuration aligned to [117] ZA is shown in Figure 4 (b),
204
demonstrating that the downward section is dominated by periodic twinning. The twinning
205
is clearly seen as a contrast difference in Figure 4 (b), and is also observable as
206
roughness of the downward section in Figure 4 (a).
ACS Paragon Plus Environment
16
Page 17 of 50 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Nano Letters
207 208
Figure 4. Type 2 downward growth of a GaAs NW. (a) [110] ZA image of a type 2 structure with
209
downward section grown for 20 min shows the defect-free vertical section, with a single twin in
210
the tip of the NW (SAED 1). (b) In [117] ZA image of a structure with 20 min downward growth,
ACS Paragon Plus Environment
17
Nano Letters 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 18 of 50
211
periodic twinning of the horizontal section is witnessed, corresponding to SAED 4. The evolution
212
of type 2 structures during the downward growth is described in more detail in the SI.
213
As type 1 structures grow precisely in the same horizontal plane (see the SI) and exhibit
214
only a single twin plane, whereas type 2 structures consist of a periodic twinning
215
superlattice, we carefully optimized the yield of higher quality type 1 structures. We
216
studied the effects of the NW density, annealing time, V/III BEP ratio during the resumed
217
growth and NW diameter on the populations of type 1 and 2 NWs. For the annealing time,
218
V/III BEP ratio and NW density, all horizontal sections were grown on similar vertical NWs.
219
The effect of each growth parameter was studied independently using the intermediate
220
values of the other two parameters (the NW density = 3×107 cm-2, the annealing time =
221
45 s, the V/III BEP ratio = 9). For the diameter series, the vertical growth time was varied
222
in order to tune the size of the initial NWs (at a fixed V/III BEP ratio). The populations
223
were characterized by analyzing top-view SEM images as described in more detail in the
224
SI.
ACS Paragon Plus Environment
18
Page 19 of 50 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Nano Letters
225
According to Figure 5 (a), increasing the NW surface density from 2.4×107 cm-2 to
226
2.5×108 cm-2 allowed us to increase the yield of type 1 structures from 20 to 100% . The
227
effect of the annealing time is shown in Figure 5 (b). Very importantly, 99% yield of type
228
1 structures was obtained with the longest annealing time of 70 s. For the shortest
229
annealing time of 20 s, the horizontal growth was mostly suppressed by the formation of
230
arbitrarily shaped bulges, showing that 20 s is not an adequate time for the deterministic
231
switching of the NW growth direction. Figure 5 (c) shows that altering the V/III ratio as the
232
growth is resumed after the annealing step also had a significant effect on the yield of
233
type 1 structures. For the lowest V/III ratio, all horizontal sections nucleated as type 1
234
structures. However, for 35% of these structures the droplets wetted the horizontal NW
235
sidewalls, terminating the original type 1 growth. Formation of these structures, referred
236
to as type 1b in the Figure 5 (e), is explained in the SI, where the top facets of such
237
structures are analyzed in more detail based on SEM images. A higher V/III ratio of 11
238
produced up to 70% yield of type 1 structures. However, many droplets started shrinking
239
during the subsequent horizontal growth, implying that such growth would eventually be
240
terminated due to the droplet consumption. Furthermore, 40% of type 2 structures
ACS Paragon Plus Environment
19
Nano Letters 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 20 of 50
241
obtained with V/III=11 exhibited growth directly downward along the sidewalls of vertical
242
NWs. These structures have nucleated similarly to type 2 NWs, and are referred to as
243
type 2b in Figure 5 (e). The SEM analysis of these structures is given in the SI. No droplets
244
were observed on top of type 2b structures.
245
Figure 5 (d) shows the effect of the NW diameter on the yield of type 1 structures. For
246
the narrowest NWs with the diameters of 75 nm, more than 99% yield of type 1 structures
247
is achieved. Increasing the NW diameter leads to a rapid decrease of the type 1
248
population. For 84 nm diameter NWs, the type 1 yield becomes only 17.4%, and drops
249
below 10% for 91 nm diameter NWs. The additional data point for 90 nm diameter NWs
250
but with the annealing time increased from 45 s to 70 s demonstrates that type 1 yield
251
increases from less than 10% to 55% despite the large NW diameter. Therefore,
252
increasing the annealing time has a similar effect as decreasing the NW diameter, both
253
leading to higher yield of type 1 structures. This will be important in what follows. Figure
254
5 (f) shows a SEM image of the high density sample with 100% yield of type 1 NWs.
ACS Paragon Plus Environment
20
Page 21 of 50 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Nano Letters
255 256
Figure 5. Effect of the growth parameter tuning on the yield of type 1 structures: (a) NW
257
density, (b) annealing time, (c) V/III BEP ratio, and (d) NW diameter. Note that the
258
intermediate data in histograms (a)–(c) are from the same sample. The inset in (b) shows
259
the typical random bulge formed when the annealing time is too short. The 30° tilted view
260
SEM images in (e) show type 1b and 2b structures as described in the text and SI. The
261
scale bars are 100 nm. (f) 30° tilted SEM image of the high density sample with 100%
262
yield of type 1 structures. (g) the NW diameter dependence of the type 1 and 2
263
populations at a fixed annealing time of 45 s (with a lower density of surface structures of
264
1.26 108 cm-2, and a higher density of 1.91 108 cm-2), fitted by the model described
265
below.
ACS Paragon Plus Environment
21
Nano Letters 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 22 of 50
266
We now compare these results with the previously published data. The droplet-NW
267
interface reshaping shown in Figure 1 (e) and analyzed in Figure 2 was observed in our
268
previous work [22]. However, as these samples were immediately cooled down after the NW
269
growth, the effect was not reproducible until the annealing step was introduced to achieve the
270
deterministic switching of the NW growth direction as described above. Similar effect of the
271
growth interface reshaping has previously been reported for Be-doped self-catalyzed GaAs NWs
272
in Ref. [27], where Be was thought to lower the droplet surface energy and to cause a partial
273
wetting of the NW sidewalls. In Ref. [28], the Ga flux was provided for 20 to 60 s after termination
274
of the As input in order to inflate the droplet and let it wet the NW side facets. The multiple (111)
275
facets observed in Ref. [27] form a similar structure to the one shown in Figure 2 (a). Similarly in
276
Ref. [28], the (111)A facet dominated the reshaped droplet-NW interface, even though a few twin
277
planes were formed above the droplets, one of which extended to the droplet-NW interface. This
278
extended twin plane is likely to represent the very first steps of nucleation toward type 1 structure.
279
Thus, prior observations support the repeatability and generality of the (111)-dominated droplet-
280
NW interface reshaping upon the growth interruption.
281
In addition to the reshaped (111)A [(1-1-1) in Figure 2 (a)] facet, our NWs comprise a (100)
282
facet, below which we always observe a (111)B facet [such as the (0-10) and (-111) facets in Figure
283
2 (b)]. The reshaped (100) facet and the (111)B facet below it were not observed in Refs. [27, 28].
284
Based on the droplets tilting symmetrically in between the (1-1-1) and (0-10) facets [away from
285
the (-110) NW side facet in Figure 2 (c)], and taking into account the interface configuration
286
observed on the NWs with the droplets removed, we conclude that the reshaped droplet-NW
287
interface consists of a combination of the (111)A and (100) facets, as illustrated in Figure 2 (e)–
ACS Paragon Plus Environment
22
Page 23 of 50 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Nano Letters
288
(h). According to this view, type 1 and type 2 structures nucleate from NWs having very similar
289
droplet-NW interfaces. However, higher quality horizontal type 1 structures are dominated by the
290
(111)A facets. Lower quality downward type 2 structures are dominated by the (100) facets and
291
grow perpendicular to the (111)B facet situated below the (100) one. The difference between type
292
1 and 2 structures should then be explained by the fine tuning of the interface geometry, namely
293
the probabilities of forming the (111)A and (100) reshaped facets. The reshaping of the growth
294
interface should be due to an interplay of the surface energetics and kinetics, supported by the fact
295
that the populations of type 1 and 2 structures can be tuned by the growth parameters and the NW
296
diameters as shown in Figure 5.
297
We now present a model to explain and quantify the switching mechanism. According
298
to Refs. [29,30], B-aligned self-catalyzed GaAs NWs and even Au-catalyzed GaAs
299
NWs grown under Ga-rich conditions exhibit a truncated growth interface with an inward
300
tapered facet wetted by a catalyst droplet. Such truncated NWs have pure ZB crystal
301
phase because nucleation occurs away from the triple phase line where solid, liquid and
302
vapor phases meet [29–32]. Unfortunately, in-situ TEM measurements [29,31] cannot
303
identify the exact orientation of the small truncated facet due to the complex structure of
304
the truncation and its fast oscillations. However, it seems reasonable that the low index
305
(111)A and (100) can both be present in the initially truncated vertical NWs as well as in
306
NWs reshaping under annealing.
ACS Paragon Plus Environment
23
Nano Letters 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
307
Page 24 of 50
According to the model of Tersoff [31], the free energy change of forming an inclined
308
facet making the angle i to the vertical, of height y and length L , is given by
309
tan i 2 y Gi L ai y bi 2 35 .
310
This expression presents the free energy relative to the vertical facet and planar growth
311
interface. Here, ai is the surface energy change upon forming the inclined facet, which
312
becomes negative at large enough contact angles of the droplet ( 133° in our
313
vertical NWs), is the chemical potential difference per GaAs pair in liquid and solid,
314
35 0.0452 nm3 is the elementary volume of GaAs pairs in solid, and bi is a positive
315
constant which determines the facet size when 0 . The energetically preferred facet
316
heigth y*( i ) that minimizes Gi is given by y*(i ) ai /[2bi (1 i )] , with i tan i /(235bi ) .
317
According to our assumption, ai 0 for both (111)A and (100) facets, with the probability
318
of their occurrence detemining the populations of type 1 ( i 1) or 2 ( i 2 ) bent NW
319
structures. We should now compare the probabilities of forming type 1 or 2 facets at
320
varying chemical potential which decreases in the annealing stage upon the growth
321
interrupt.
(1)
ACS Paragon Plus Environment
24
Page 25 of 50 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
322
323 324
325
Nano Letters
The minimum free energy values at y y*(i ) are given by
G*(i )
ai L 4bi (1 i ) .
(2)
The probability p1 of forming type 1 structure can generally be put as
p1
exp(G1* / k BT ) exp(G1* / k BT ) exp(G2* / k BT ) ,
(3)
326
with T as the growth temperature and k B as the Boltzmann constant. As shown in the SI,
327
chemical potential decreases with the annealing time t approximatelly as
k BT 33 h 1 k35 0 35 f ( ) R R,
328
0 (1 t )
329
with 0 as the initial chemical potential value at t 0 . The constant determines the
330
rate of chemical potential decrease, with 3 0.02 nm3 as the elementary volume of liquid
331
Ga,
,
h 0.326
nm
as
the
(4)
height
of
GaAs
monolayer,
332
f ( ) (1 cos )(2 cos ) /[(1 cos ) sin ] as the geometrical function of the droplet
333
contact angle , k35 as the crystallization rate of GaAs pairs, and R as the NW radius
334
(which equals the radius of the droplet base). Chemical potential decreases linearly with
335
t , while for a given t it is higher for larger R because larger droplets deplete more slowly
ACS Paragon Plus Environment
25
Nano Letters 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 26 of 50
336
with their As. Using equations (2) to (4), the yield of type 1 structures is obtained in the
337
form p1
338
1 1 u 1 exp 1 2 0 (1 t ) 1 1 0 (1 t ) ,
(5)
339
with [a22 /(4b2 )]( L / k BT ) and u a12b2 /(a22b1 ) .
340
Using the plausible parameters of self-catalyzed growth of GaAs NWs ( 0 0.2 eV
341
[33,34], k35 =165 s-1 corresponding to the mean axial growth rate of our vertical NWs of
342
1.06 nm/s [22], and 133o), we obtain the values on the order of 1 min-1 for R ~ 50
343
nm, showing that chemical potential tends to zero after ~ 1 min of annealing. According
344
to Figures 5 (b) and (d), an almost 100% yield of type 1 NW structures is obtained after
345
70 s annealing and even after 45 s annealing for a smaller NW diameter of 75 nm. Shorter
346
annealing times or larger NW diameters favor type 2 structures, which becomes
347
predominant (more than 90%) for the largest NW diameters of 90–91 nm. According to
348
the above analysis, smaller diameters or longer annealing times bring the VLS system
349
closer to the quasi-equilibrium state at 0 , corresponding to t 1 in equation (5).
350
On the other hand, higher favors type 2 structures. While the i and u parameters
ACS Paragon Plus Environment
26
Page 27 of 50 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Nano Letters
351
entering equation (5) are unknown, higher yield of type 2 structures at 0 (and
352
therefore the preference of the (100) truncation in vertical NWs), transitioning to an almost
353
100% yield of type 1 structures at 0 requires that
354
1 2 0 u 1 u 1 , 1 1 0 ,
355
implying that 1 2 . These two inequalities are essential for describing the observed
356
trends in the two competing NW structures under annealing.
(6)
357
Using equation (6), we can quantify the yield of type 1 structures versus the NW
358
diameter at a fixed t of 45 s. The facet length L entering the parameter should be
359
proportional to R . We can then write R / R1 and t R0 / R according to equation (5).
360
This gives p1 ( R)
361
1 R 1 u 1 exp R 1 ( 1 R / R ) 1 ( 1 R / R ) 2 0 0 1 0 0 . 1
(7)
362
Figure 5 (g) shows a good fit to the data by equation (7) with R1 1.5 nm, R0 32.5 nm,
363
u 2 , 2 0 1 and 10 7. It is seen that the transition from less than 10% to almost
ACS Paragon Plus Environment
27
Nano Letters 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 28 of 50
364
100% of type 1 structures is very sharp and occurs for a relatively small diameter change
365
from 90 to 75 nm.
366
Very importantly, all the statistical data on type 1 versus type 2 NW structures shown in
367
Figures 5 (a) to (d) are qualitatively explained within our model. As discussed above,
368
longer annealing times and smaller NW sizes decrease chemical potential and hence
369
favor type 1 structures. Higher density NWs are ~ 100 nm longer and thinner (71 nm in
370
diameter) than the sparse ones (82 nm in diameter). Therefore, the NW density effect is
371
the same as for the diameter series. Due to a higher fraction of re-emitted As species
372
[33], the local V/III flux ratio should be higher for denser NWs. Higher As flux is known to
373
increase the axial NW growth rate and simultaneously shrink the Ga droplets, yielding
374
thinner NWs [35–37]. Lower V/III BEP ratios leads to a steeper decrease of chemical
375
potential in the gallium droplets [33, 34] and hence favor a faster formation of type 1
376
structures when the growth is resumed after annealing. The only exception from this trend
377
is the case of the highest V/III BEP ratio of 11 [see Fig. 5 (c)], where the population of
378
type 1 structures increases even though a higher is expected. This may be associated
379
with shorter incubation times, where more energetically preferred structures are formed
ACS Paragon Plus Environment
28
Page 29 of 50 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Nano Letters
380
over a given period of time. It should also be noted that nucleating the horizontal growth
381
with an optimized V/III BEP ratio for each density (for example, V/III=7 for the intermediate
382
NW density) and then tuning the V/III ratio back to 9 could produce 100% yield of type 1
383
structures. This gives additional versatility of the growth parameters that can individually
384
be tuned to maximize the deterministic nucleation of type 1 structures.
385
Based on the structural analysis of the reshaped droplet-NW interfaces and type 1
386
structures shown in Figures 2 and 3, type 1 structures nucleate on the (1-1-1) facet
387
marked in Figure 2 (a). Simultaneously a twin plane forms, creating a (111)B facet to
388
oppose the (1-1-1) one. Because this twin plane is observed in both types of structures,
389
it is most likely initiated by the triple phase line nucleation at the droplet edge opposing
390
the reshaped (1-1-1) and (0-10) facets, where the droplet contact angle is less than 90°
391
[29, 32]. In type 1 structures, the twin plane between the (111)A and (111)B facets pins
392
the droplet, allowing the growth to propagate in the direction. Such mechanism is
393
known as the twin-mediated growth, observed previously for Ge ingots and Au-catalyzed
394
Ge and GaInP NWs. [38–42] However, our growth mode is different from previous
395
observations. In our case, two different interface configurations are observed, where the
ACS Paragon Plus Environment
29
Nano Letters 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 30 of 50
396
flat facet dominating the droplet-NW interface may be either the upper B-polar [Figure 3
397
(c)], or the lower A-polar facet [Figure 3 (d)], and the other (111) facet is replaced by
398
several smaller microfacets. These two morphologies present different phases of a novel
399
type of twin-mediated growth where the flat facet dominating the growth varies
400
periodically. Oscillations between the flat (111)A and (111)B facets during growth is
401
supported by the periodically changing morphology of the top parts of horizontal NWs,
402
where one half-period is almost parallel to the twin plane and the other has a downward
403
slope with respect to the twin. This fine structure can readily be seen in SEM images
404
shown in Figure 1 (f) and in the SI, and in more detail in the side-view TEM in Figures 3
405
(c) and (d). The sustainability of this oscillating twin-mediated growth mode for long
406
horizontal sections is demonstrated in the SI by analyzing the horizontal growth rate for
407
a V/III BEP ratio of 9. The growth rate remains constant for at least 20 min and equals the
408
axial growth rate of vertical NWs (1.06 nm/s).
409
As regards the surface energetics of horizontal growth, we speculated that the (111)A
410
facets are energetically preferred to all other types of facets at low enough chemical
411
potentials, which is why they are most representative in the reshaped droplet-NW
ACS Paragon Plus Environment
30
Page 31 of 50 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Nano Letters
412
interface. On the other hand, it is known that the (111)B plane of GaAs has a lower energy
413
than the (111)A one (0.69 J/m2 against 0.82 J/m2 in contact with As-rich vapors according
414
to Ref. [43]). The same property should pertain when these facets are in contact with the
415
Ga liquid, consistent with the fact that the usual NW growth direction is B [44]. Our
416
type 1 structures nucleate on a (111)A facet, which is inward tapered for vertical NWs
417
and has a lower effective surface energy with respect to the outward tapered (111)B facet
418
[30]. The situation changes after nucleation of a horizontal NW section, where the
419
energetically preferred facet to introduce is the (111)B one, which allows for the stable
420
horizontal growth of type 1 NWs. This explains the unique growth mode whereby the
421
horizontal growth direction is maintained by alternating the (111)A and (111)B facets, and
422
should work equally well for other III-V NWs.
423
In conclusion, we have demonstrated a high level of control over the growth direction
424
of self-catalyzed GaAs NWs and found a novel type of twin-mediated growth mode, where
425
the growth interface oscillates between the two flat (111) facets with different polarity. By
426
controlling the NW density, annealing time, V/III ratio during the horizontal growth, and
427
the NW diameter, we are able to obtain 100% yield of regular 90° bent NW structures, in
ACS Paragon Plus Environment
31
Nano Letters 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 32 of 50
428
which all the horizontal sections start at the pre-determined height. Our model describes
429
an interesting interplay between the surface energetics and growth kinetics, whereby the
430
horizontal growth is preferred at low chemical potentials achieved in the annealing stage.
431
It explains all the observed data and predicts that such morphology should be achievable
432
for any VLS III-V NWs whose growth front is initially truncated. Detailed structural
433
investigations reveal high crystal quality of the obtained structures, which makes them
434
extremely promising for quantum electronic and photonic applications.
435
ASSOCIATED CONTENT
436
Supporting Information contains: SEM analysis of NW top faceting; Additional SEM
437
images to support statistical analysis of type 1 and 2 populations; Description of different
438
structures found on the sample; Analysis of horizontal growth rate; Evolution of type 2
439
downward growth; Additional SEM analysis of growth interface during continued growth;
440
Additional SEM images of exceptions from type 1 and 2 growth due to short annealing or
441
non-optimal V/III BEP ratio; TEM analysis of NWs prior to annealing; Illustrative SEM
ACS Paragon Plus Environment
32
Page 33 of 50 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Nano Letters
442
images of the horizontal plane on which type 1 growth occurs; and Derivation of the
443
chemical potential decrease under annealing.
444
AUTHOR INFORMATION
445
Corresponding Author
446
* Email:
[email protected] 447
Author Contributions
448
The manuscript was written through contributions of all authors. All authors have given
449
approval to the final version of the manuscript.
450
ACKNOWLEDGMENT
451
This work made use of Aalto University Nanomicroscopy Center (Aalto-NMC) and
452
Tampere University of Technology Microscopy center facilities. E.K, T.H and M.G
453
acknowledge financial support from the Academy of Finland projects NESP (decision No.
454
294630), NanoLight (decision 310985) and the Vilho, Yrjö and Kalle Väisälä Foundation
455
of the Finnish Academy of Science and Letters. H.V.A.G and Y.G.G. acknowledge
ACS Paragon Plus Environment
33
Nano Letters 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 34 of 50
456
financial support from São Paulo Research Foundation, FAPESP (decisions grant
457
numbers 14/50513-7 and 16/10668-7). V.G.D. acknowledges the Ministry of Education
458
and Science of the Russian Federation for financial support under grant 14.587.21.0040
459
(project ID RFMEFI58717X0040).
460
REFERENCES
461
[1] B. Mayer, L. Janker, B. Loitsch, J. Treu, T. Kostenbader, S. Lichtmannecker, T.
462
Reichert, S. Morkötter, M. Kaniber, G. Abstreiter, C. Gies, G. Koblmüller, J.J. Finley,
463
Monolithically Integrated High-β Nanowire Lasers on Silicon, Nano Letters, Vol. 16, Iss.
464
1, 2016, pp. 152-156, DOI: 10.1021/acs.nanolett.5b03404
465
[2] K. Tomioka, J. Motohisa, S. Hara, K. Hiruma, T. Fukui, GaAs/AlGaAs Core Multishell
466
Manowire-Based Light-Emitting Diodes on Si, Nano Letters, Vol. 10, Iss. 5, 2010, pp.
467
1639-1644, DOI: 10.1021/nl9041774
468
[3] C. Patrik, T. Svensson, T. Mårtensson, J. Trägårdh, C. Larsson, M. Rask, D.
469
Hessman, L. Samuelson, J. Ohlsson, Monolithic GaAs/InGaP nanowire light emitting
ACS Paragon Plus Environment
34
Page 35 of 50 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Nano Letters
470
diodes on silicon, Nanotechnology, Vol. 19, Iss. 30, 2008, pp. 305201, DOI:
471
https://doi.org/10.1088/0957-4484/19/30/305201
472
[4] J. Wallentin, N. Anttu, D. Asoli, M. Huffman, I. Åberg, M.H. Magnusson, G. Siefer, P.
473
Fuss-Kailuweit, F. Dimroth, B. Witzigmann, H.Q. Xu, L. Samuelson, K. Deppert, M.T.
474
Borgström, InP nanowire array solar cells achieving 13.8% efficiency by exceeding the
475
ray optics limit, Science, Vol. 339, 2013, https://doi.org/10.1126/science.1230969
476
[5] S. Gazibegovic, D. Car, H. Zhang, S.C. Balk, J.A. Logan, M.W.A. de Moor, M.C.
477
Cassidy, R. Schmits, D. Xu, G. Wang, P. Krogstrup, R.L.M. Op het Veld, K. Zuo, Y. Vos,
478
J. Shen, D. Bouman, B. Shojaei, D. Pennachio, J.S. Lee, P.J. van Veldhoven, S. Koelling,
479
M.A. Verheijen, L.P. Kouwenhoven, C.J. Palmstrøm, E.P.A.M Bakkers, Epitaxy of
480
advanced nanowire quantum devices, Nature, Vol. 548, 2017, pp. 434 , DOI:
481
http://dx.doi.org/10.1038/nature23468
482
[6] J. Kang, Y. Cohen, Y. Ronen, M. Heiblum, R. Buczko, P. Kacman, R. Popovitz-Biro,
483
H. Shtrikman, Crystal Structure and Transport in Merged InAs Nanowires MBE Grown on
ACS Paragon Plus Environment
35
Nano Letters 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
484
(001)
InAs,
Nano
Letters,
Vol.
485
http://dx.doi.org/10.1021/nl402571s
13,
Iss.
Page 36 of 50
11,
2013,
pp.
5190-5196,
DOI:
486
[7] F. Krizek, T. Kanne, D. Razmadze, E. Johnson, J. Nygård, C.M. Marcus, P.
487
Krogstrup, Growth of InAs Wurtzite Nanocrosses from Hexagonal and Cubic Basis, Nano
488
Letters,
489
http://dx.doi.org/10.1021/acs.nanolett.7b02604.
Vol.
17,
Iss.
10,
2017,
pp.
6090-6096,
DOI:
490
[8] T. Rieger, D. Rosenbach, D. Vakulov, S. Heedt, T. Schäpers, D. Grützmacher, M.I.
491
Lepsa, Crystal Phase Transformation in Self-Assembled InAs Nanowire Junctions on
492
Patterned Si Substrates, Nano Letters, Vol. 16, Iss. 3, 2016, pp. 1933-1941, DOI:
493
10.1021/acs.nanolett.5b05157
494
[9] D. Dalacu, A. Kam, D.G. Austing, P.J. Poole, Droplet Dynamics in Controlled InAs
495
Nanowire Interconnections, Nano Letters, Vol. 13, Iss. 6, 2013, pp. 2676-2681, DOI:
496
10.1021/nl400820w
497 498
[10] H. Potts, N.P. Morgan, G. Tütüncüoglu, M. Friedl, A. Fontcuberta, i Morral, Tuning growth
direction
of
catalyst-free
InAs(Sb)
nanowires
with
indium
droplets,
ACS Paragon Plus Environment
36
Page 37 of 50 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Nano Letters
499
Nanotechnology, Vol. 28, Iss. 5, 2017, pp. 054001, DOI: https://doi.org/10.1088/1361-
500
6528/28/5/054001
501
[11] Y. Luo, C. Chi, M. Jiang, R. Li, S. Zu, Y. Li, Z. Fang, Plasmonic Chiral
502
Nanostructures: Chiroptical Effects and Applications, Advanced Optical Materials, Vol. 5,
503
Iss. 16, 2017, pp. 1700040 DOI: 10.1002/adom.201700040
504
[12] G. Leahu, E. Petronijevic, A. Belardini, M. Centini, C. Sibilia, T. Hakkarainen, E.
505
Koivusalo, M. Rizzo Piton, S. Suomalainen, M. Guina, Evidence of Optical Circular
506
Dichroism in GaAs-Based Nanowires Partially Covered with Gold, Advanced Optical
507
Materials, Vol. 5, 2017, pp. 1601063, DOI: 10.1002/adom.201601063
508
[13] E. Petronijevic, M. Centini, A. Belardini, G. Leahu, T. Hakkarainen, C. Sibilia, Chiral
509
near-field manipulation in Au-GaAs hybrid hexagonal nanowires, Optics Express, Vol. 25,
510
Iss. 13, 2017, pp. 14148-14157, DOI: 10.1364/OE.25.014148
511
[14] A. Kelrich, O. Sorias, Y. Calahorra, Y. Kauffmann, R. Gladstone, S. Cohen, M.
512
Orenstein, D. Ritter, InP Nanoflag Growth from a Nanowire Template by in Situ Catalyst
ACS Paragon Plus Environment
37
Nano Letters 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
513
Manipulation,
Nano
Letters,
514
10.1021/acs.nanolett.6b00648
Vol.
16,
Iss.
Page 38 of 50
4,
2016,
pp.
2837-2844,
DOI:
515
[15] J. Wang, S. Plissard, M.A. Verheijen, L. Feiner, A. Cavalli, Bakkers, Erik P. A. M.,
516
Reversible Switching of InP Nanowire Growth Direction by Catalyst Engineering, Nano
517
Letters, Vol. 13, Iss. 8, 2013, pp. 3802-3806, DOI: 10.1021/nl401767b
518
[16] S. Conesa-Boj, E. Russo-Averchi, A. Dalmau-Mallorqui, J. Trevino, E.F. Pecora, C.
519
Forestiere, A. Handin, M. Ek, L. Zweifel, L.R. Wallenberg, D. Rüffer, M. Heiss, D. Troadec,
520
L. Dal Negro, P. Caroff, A. Fontcuberta, i Morral, Vertical “III–V” V-Shaped
521
Nanomembranes Epitaxially Grown on a Patterned Si[001] Substrate and Their
522
Enhanced Light Scattering, ACS Nano, Vol. 6, Iss. 12, 2012, pp. 10982-10991, DOI:
523
10.1021/nn304526k
524
[17] M. de la Mata, R. Leturcq, S. Plissard, C. Rolland, C. Magén, J. Arbiol, P. Caroff,
525
Twin-Induced InSb Nanosails: A Convenient High Mobility Quantum System, Nano
526
Letters, Vol. 16, Iss. 2, 2016, pp. 825-833, DOI: 10.1021/acs.nanolett.5b05125
ACS Paragon Plus Environment
38
Page 39 of 50 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Nano Letters
527
[18] F. Lenrick, M. Ek, K. Deppert, L. Samuelson, L.R. Wallenberg, Straight and kinked
528
InAs nanowire growth observed in situ by transmission electron microscopy, Nano
529
Research, Vol. 7, Iss. 8, 2014, pp, DOI: https://doi.org/10.1007/s12274-014-0481-4.
530
[19] K. Hillerich, K.A. Dick, C. Wen, M.C. Reuter, S. Kodambaka, F.M. Ross, Strategies
531
To Control Morphology in Hybrid Group III–V/Group IV Heterostructure Nanowires, Nano
532
Letters, Vol. 13, Iss. 3, 2013, pp. 903-908, DOI: 10.1021/nl303660h
533
[20] T.V. Hakkarainen, A. Schramm, J. Mäkelä, P. Laukkanen, M. Guina, Lithography-
534
free oxide patterns as templates for self-catalyzed growth of highly uniform GaAs
535
nanowires
536
4484/26/27/275301
on
Si(111),
Nanotechnology,
Vol.
26,
2015,
DOI:
10.1088/0957-
537
[21] E. Koivusalo, T. Hakkarainen, M. Guina, Structural Investigation of Uniform
538
Ensembles of Self-Catalyzed GaAs Nanowires Fabricated by a Lithography-Free
539
Technique, Nanoscale Research Letters, Vol. 12, Iss. 1, 2017, pp. 192, DOI:
540
10.1186/s11671-017-1989-9
ACS Paragon Plus Environment
39
Nano Letters 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 40 of 50
541
[22] E.S. Koivusalo, T.V. Hakkarainen, M.D. Guina, V.G. Dubrovskii, Sub-Poissonian
542
Narrowing of Length Distributions Realized in Ga-Catalyzed GaAs Nanowires, Nano
543
Letters, Vol. 17, Iss. 9, 2017, pp. 5350-5355, DOI: 10.1021/acs.nanolett.7b01766
544
[23] C. Colombo, D. Spirkoska, M. Frimmer, G. Abstreiter, A. Fontcuberta, i Morral, Ga-
545
assisted catalyst-free growth mechanism of GaAs nanowires by molecular beam epitaxy,
546
Physical Review B. Vol. 77, 2008, pp. 155326 DOI: 10.1103/PhysRevB.77.155326
547
[24] E. Uccelli, J. Arbiol, C. Magen, P. Krogstrup, E. Russo-Averchi, M. Heiss, G.
548
Mugny, F. Morier-Genoud, J. Nygård, J.R. Morante, A. Fontcuberta, i Morral, Three-
549
Dimensional Multiple-Order Twinning of Self-Catalyzed GaAs Nanowires on Si
550
Substrates, Nano Letters, Vol. 11, Iss. 9, 2011, pp. 3827-3832, DOI: 10.1021/nl201902w
551
[25] X. Yuan, P. Caroff, J. Wong-Leung, L. Fu, H.H. Tan, C. Jagadish, Tunable Polarity
552
in a III–V Nanowire by Droplet Wetting and Surface Energy Engineering, Advanced
553
Materials, Vol. 27, Iss. 40, 2015, pp. 6096-6103, DOI: 10.1002/adma.201503540
ACS Paragon Plus Environment
40
Page 41 of 50 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Nano Letters
554
[26] B. Wacaser, K. Deppert, L. Karlsson, L. Samuelson and W. Seifert, Growth and
555
characterization of defect free GaAs nanowires, Journal of Crystal Growth, Vol. 27, Iss.
556
2, 2006, pp. 504-508, DOI: //doi.org/10.1016/j.jcrysgro.2005.11.075
557
[27] Y. Zhang, Z. Sun, A.M. Sanchez, M. Ramsteiner, M. Aagesen, J. Wu, D. Kim, P.
558
Jurczak, S. Huo, L.J. Lauhon, H. Liu, Doping of Self-Catalyzed Nanowires under the
559
Influence of Droplets, Nano Letters, Vol. 18, Iss. 1, 2017, pp. 81-87, DOI:
560
10.1021/acs.nanolett.7b03366
561
[28] L. Li, D. Pan, X. Yu, H. So, J. Zhao, Manipulation of morphology and structure of
562
the top of GaAs nanowires grown by molecular-beam epitaxy, Journal of Semiconductors,
563
Vol. 38, Iss. 10, 2017, pp. 103001, DOI: https://doi.org/10.1088/1674-4926/38/10/103001
564
[29] D. Jacobsson, F. Panciera, J. Tersoff, M.C. Reuter, S. Lehmann, S. Hofmann, K.A.
565
Dick, F.M. Ross, Interface dynamics and crystal phase switching in GaAs nanowires,
566
Nature, Vol. 531, 2016, pp. 317 DOI: http://dx.doi.org/10.1038/nature17148
ACS Paragon Plus Environment
41
Nano Letters 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 42 of 50
567
[30] V.G. Dubrovskii, Development of Growth Theory for Vapor–Liquid–Solid
568
Nanowires: Contact Angle, Truncated Facets, and Crystal Phase, Crystal Growth &
569
Design, Vol. 17, Iss. 5, 2017, pp. 2544-2548, DOI: 10.1021/acs.cgd.7b00076
570
[31] C.-Y. Wen, J. Tersoff, K. Hillerich, M.C. Reuter, J.H. Park, S. Kodambaka, E.A.
571
Stach, F.M. Ross, Periodically Changing Morphology of the Growth Interface in Si, Ge,
572
and GaP Nanowires, Physical Review Letters, Vol. 107, Iss. 2, 2011, pp. 025503, DOI:
573
https://doi.org/10.1103/PhysRevLett.107.025503
574
[32] F. Glas, J. Harmand, G. Patriarche, Why does wurtzite form in nanowires of III-V
575
zinc blende semiconductors? Phys Rev Lett, Vol. 99, Iss. 14, 2007, pp. 146101, DOI:
576
10.1103/PhysRevLett.99.146101
577
[33] F. Glas, M.R. Ramdani, G. Patriarche, J. Harmand, Predictive modeling of self-
578
catalyzed III-V nanowire growth, Physical Review B, Vol. 88, Iss. 19, 2013, pp. 195304,
579
DOI: https://doi.org/10.1103/PhysRevB.88.195304
ACS Paragon Plus Environment
42
Page 43 of 50 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Nano Letters
580
[34] V.G. Dubrovskii, Group V sensitive vapor–liquid–solid growth of Au-catalyzed and
581
self-catalyzed III–V nanowires, in: Journal of Crystal Growth, Vol. 440, Iss. 15, 2016, pp.
582
62–68, DOI: https://doi.org/10.1016/j.jcrysgro.2016.01.019
583
[35] T. Rieger, S. Heiderich, S. Lenk, M.I. Lepsa, D. Grützmacher, Ga-assisted MBE
584
growth of GaAs nanowires using thin HSQ layer, Journal of Crystal Growth, Vol. 353, Iss.
585
1, 2012, pp. 39-46. DOI: https://doi.org/10.1016/j.jcrysgro.2012.05.006
586
[36] M.R. Ramdani, J.C. Harmand, F. Glas, G. Patriarche, L. Travers, Arsenic Pathways
587
in Self-Catalyzed Growth of GaAs Nanowires, Crystal Growth & Design, Vol. 13, Iss. 1,
588
2013, pp. 91-96, DOI: 10.1021/cg301167g
589
[37] M. Federico, V.G. Dubrovskii, D. Rüffer, G. Tütüncüoğlu, Y. Fontana, A.
590
Fontcuberta, i Morral, Tailoring the diameter and density of self-catalyzed GaAs
591
nanowires on silicon, Nanotechnology, Vol. 26, Iss. 10, 2015, pp. 105603, DOI:
592
https://doi.org/10.1088/0957-4484/26/10/105603
ACS Paragon Plus Environment
43
Nano Letters 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 44 of 50
593
[38] E. Billig, Growth of monocrystals of germanium from an undercooled melt,
594
Proceedings of the Royal Society of London.Series A.Mathematical and Physical
595
Sciences, Vol. 229, Iss. 1178, 1955, pp. 346-363, DOI: 10.1098/rspa.1955.0090
596
[39] D.R. Hamilton, R.G. Seidensticker, Propagation Mechanism of Germanium
597
Dendrites, Journal of Applied Physics, Vol. 31, Iss. 7, 1960, pp. 1165-1168 DOI:
598
10.1063/1.1735796
599
[40] A.J. Shahani, P.W. Voorhees, Twin-mediated crystal growth, Journal of Materials
600
Research,
Vol.
31,
Iss.
601
https://doi.org/10.1557/jmr.2016.308
19,
2016,
pp.
2936-2947,
DOI:
602
[41] A.D. Gamalski, P.W. Voorhees, C. Ducati, R. Sharma, S. Hofmann, Twin Plane Re-
603
entrant Mechanism for Catalytic Nanowire Growth, Nano Letters, Vol. 14, Iss. 3, 2014,
604
pp. 1288-1292, DOI: 10.1021/nl404244u
605
[42] D.S. Oliveira, L.H.G. Tizei, A. Li, T.L. Vasconcelos, C.A. Senna, B.S. Archanjo, D.
606
Ugarte, M.A. Cotta, Interaction between lamellar twinning and catalyst dynamics in
ACS Paragon Plus Environment
44
Page 45 of 50 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Nano Letters
607
spontaneous core–shell InGaP nanowires, Nanoscale, Vol. 7, Iss. 29, 2015, pp. 12722-
608
12727, DOI: 10.1039/C5NR02747K
609
[43] N. Moll, A. Kley, E. Pehlke, M. Scheffler, GaAs equilibrium crystal shape from first
610
principles, Physical Review B, Vol. 54, Iss. 12, 1996, pp. 8844-8855, DOI:
611
10.1103/PhysRevB.54.8844
612
[44] W. Kim, V.G. Dubrovskii, J. Vukajlovic-Plestina, G. Tütüncüoglu, L. Francaviglia, L.
613
Güniat, H. Potts, M. Friedl, J. Leran, A. Fontcuberta i Morral, Bistability of Contact Angle
614
and Its Role in Achieving Quantum-Thin Self-Assisted GaAs nanowires, Nano Letters,
615
Vol. 18, Iss. 1, 2018, pp. 49-57, DOI: 10.1021/acs.nanolett.7b03126.
ACS Paragon Plus Environment
45
(a) Self-catalyzed NW
Page 46 of 50 (c) Continued growth nm
1 2 3 4 5 6 7 8 9 10 11 12 13 (d) 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51
Nano Letters
Annealing
20
growth
(b)
1 µm
(e)
1 µm
(f)
1 µm Type 1
ACS Paragon Plus Environment
(g)
Type 2
(a) 47 of 50 Page 20 nm
Nano Letters -- -
(111)
20 nm
(c) 20 nm
- -
-
-- -
(101)
(100)
(111)
(010)
-
(011)
-
(101)
-
(110)
-
(111)
(101
)
(e) ) (101 -110 ) ( ---
(111) (010) -(111)
(011)
(011)
1 2 -3 (111) 4 5 6 -7 (811) 8 9 10 11 ) (d) 12 -110 ( 13 14 15 16 17 50 nm 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51
(b)
-- -
(111)
-- (f) (111) -(010) (111) (g) 109.5°
ACS Paragon Plus Environment
-
(011)
(h) 125.3°
-
(101)
(b)
(a)
Nano Letters
1
Page 48 of 502
3 1 -1 -1 5 nm 5 nm 2 31 4 2 5 6 -1 7 5 nm 8 9200 nm 10 11 (c) 12 13 14 15 16 {111}B 17 18 19 20 21 22 23 24 25 nm 25 26 27 (e) (d) 28 {111}B 29 30 31 32 {111}A {111}A 25 5 nm 33 nm 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 ACS Paragon Plus Environment 49 50 51
3
(a) Page 49 of 150
Nano Letters 1
1[110] 2 3 -1 5 nm 4 5 6 7 2 8 5 1/nm 9 10 11 12 -1 50 nm 2 5 nm 13 14 15 (b) 16 17 18 [117] 19 20 21 100 nm 22 23 24 -1 5 nm 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 ACS Paragon Plus Environment 49 50 51
4
3
3
4
5 nm
-1
(b)
T ype 2
T ype 1
80
80
Yield (%)
Yield (%)
100
1 60 2 40 3 20 4 0 5 6 (c) 7 100 (c) 8 80 9 10 60 11 40 12 20 13 0 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51
T ype 2
T ype 1
100
Nano (e) Letters2b 1b (g)
60 40 20
2.4E7
0
2.5E8
3.2E7
Nanowire density (cm-2) Type 2 Type 2b
Type 1 Type 1b
20
45
70
A nnealing time (s)
(f) (d)
Type 2, 45 s Type 2, 70 s
Type 1, 45 s Type 1, 70 s
100
Yield (%)
Yield (%)
80
7
9
V/III ratio
11
Page 50 of 50
Type 1 and 2 yields (%)
(a)
100 80 Type 1, lower density Type 2, lower density Type 1, higher density Type 2, higher density
60 40 20 0
60
70
40
80
85
90
Nanowire diameter (nm)
1 μm
20 0
75
75
80
85
90
Diameter (nm)
ACS Paragon Plus Environment
95